Document Type : Original Research Paper
Graphical Abstract
Highlights
· Green synthesis of ZnO nanoparticles using leaves of Coriandrum sativum as a plant extract.
· Influence of annealing temperature on the structural, morphological, and optical properties of Coriandrum sativum leaf extract-assisted ZnO nanoparticles.
· Efficient remediation of lead (Pb), and chromium (Cr) ions, achieving removal efficiencies of 84.85% for “Pb” and 99.99% for “Cr” ions.
· Phytochemical-derived surface functionality study combined with the Langmuir and Freundlich adsorption isotherm models.
Please note: The following content displays the text-only preview. For the full article, complete with all illustrations, data tables, and equations, please download the free PDF from the sidebar at the top of this page.
1) Introduction:
The silent infiltration of heavy metal ions into water bodies has emerged as a hidden yet devastating threat to global water security. Originating from industrial discharge, mining runoff, and agricultural practices, toxic metals such as lead (Pb), cadmium (Cd), mercury (Hg), arsenic (As), and chromium (Cr) persist in the environment due to their non-biodegradable nature. [1]. This exponential rise in water pollution severely risks aquatic fauna, human health, and overall environmental stability [2]. Industrial effluents such as synthetic dyes, hydrocarbons, oils, acids, heavy metal ions, and inorganic chemical waste are particularly concerning since many of them are non-biodegradable and highly toxic [3]. The release of such hazardous compounds into aquatic ecosystems leads to long-term contamination, disrupting ecological balance. Furthermore, certain industrial discharges contain chemical-reducing agents such as ferrous salts and sulphides, which react with dissolved oxygen, depleting its availability for aquatic organisms [4]. This oxygen deficiency has a critical impact on marine biodiversity and endangers marine life. Heavy metal ions, originating from both natural geological processes and anthropogenic activities, have emerged as persistent environmental pollutants due to their bio-accumulative and toxic nature [5]. The rapid expansion of industries and agricultural sectors has further exacerbated heavy metal contamination in our natural water resources, further intensifying the associated environmental and health risks [6]. Heavy metal ions such as lead (Pb), chromium (Cr), cadmium (Cd), and arsenic (As) are of major concern due to their carcinogenic nature. Conventional techniques like filtration and distillation are ineffective in removing these toxic ions from the wastewater. At present, the adsorption technique stands out as one of the most efficient methods for the effective removal of heavy metal ions from wastewater [7]. In this technique, the pollutants, such as heavy metal ions, adhere to the surface of an adsorbent material through a chemisorption or physisorption phenomenon. With the advancement of nanotechnology and the emergence of novel nanoengineered materials, the efficiency of heavy metal ion removal and adsorption capacity has significantly improved. This enhancement is primarily attributed to the high surface area-to-volume ratio of nanomaterials, which provides a larger active surface for metal ion interaction [8, 9]. The nano size of adsorbate and controlled pore size distribution increase chemical reactivity and entrapment of pollutants, facilitating better contaminant adsorption [10,11]. A promising and eco-friendly approach within nanotechnology is green synthesis, which enables the synthesis of nanoparticles by reducing the metal precursor with phytochemicals such as flavonoids, alkaloids, terpenoids, and phenolic compounds of the natural plant-derived components, such as roots, leaves, and flowers. Among the diverse range of nanoparticles, metal oxide nanoparticles stand out as a powerful tool in environmental remediation due to their exceptional properties, including a wide band gap and high sensitivity to visible light [12-15]. According to the literature, Various plant species, including Chenopodium exsuccum [16], Camellia sinensis (Tea plant) [17], Rumex Nervosus Vahl [18], and Acacia nilotica [19], have been extensively utilized for synthesizing. An overview of recent advances in the green synthesis of metal oxide nanoparticles and their effective utilization in the remediation of heavy metal ions has been presented in Table 1.
So the goals of this research work are (a) to synthesize ZnO nanoparticles using the green synthesis route method, in which leaves of the Coriandrum sativum (Coriander) plant will be used as plant extract, (b) to study the influence of temperature on the prepared ZnO nanoparticles, (c) to made to eliminate few of the hazardous metal ions such as chromium (Cr), and lead (Pb), from the industrial wastewater by adsorption of ZnO nanoparticles, and (d) to study the adsorption mechanism of the heavy metal ions on the ZnO reactive sites.
2) Experimental:
2.1) Preparation of wastewater:
To assess heavy metal ion contaminated water, wastewater samples were collected from an industrial discharge site near Narwana, Haryana (29.5771501°N, 76.1325274°E), India. The initial samples exhibited a pale silver-grey hue with visible suspended particulate matter, as illustrated in Fig. 1(a). To eliminate coarse impurities, the samples were subjected to double-stage filtration using Whatman grade 1 filter paper (pore size: 11.0 µm). This process effectively removed the larger particulates. However, the visual appearance of the industrial wastewater remains unchanged after filtration (see Fig. 1 (b)), suggesting the presence of residual dissolved species that are not detectable by visual inspection.
2.2) Preparation of Plant Extract:
For the synthesis process, a plant-based extract was prepared using Coriandrum sativum (coriander) leaves, as shown in Fig. 2(a). Freshly harvested leaves were air-dried in a shaded area for approximately 7-10 days to prevent photodegradation. Once completely dried, the leaves were crushed using a mortar and pestle to produce a fine, uniform powder, illustrated in Fig. 2(b). An amount of 5.0 grams of this powdered material was added to 100 ml of deionized water and subjected to thermal treatment by boiling at 100°C for 20 minutes. After boiling, the solution was allowed to cool naturally to room temperature. It was then centrifuged at 6000 rpm for 10 minutes to separate any residual solids. The clear supernatant obtained post-centrifugation was collected as the Coriandrum sativum extract, and the residue was discarded. This extract was monitored for 10 days to assess its stability. Throughout the observation period, no sedimentation or phase separation was detected, confirming the formation of a stable aqueous plant extract, as depicted in Fig. 2(c).
2.3) Preparation of ZnO nanoparticles:
To synthesize ZnO nanoparticles, 0.01 mole of zinc acetate dihydrate [Zn (CH3COO)2·2H2O] was dissolved in 100 ml of deionized water, forming a 0.1 M precursor solution. The solution was maintained at 60°C on a hot plate with continuous magnetic stirring for 1 hour to ensure complete dissolution. Upon achieving a clear and homogeneous solution, 20 ml of the previously prepared plant extract was introduced gradually under constant agitation. The reaction mixture was then vigorously stirred for an additional 30 minutes to facilitate the formation of zinc oxide precursors. The resulting suspension was centrifuged at 6000 rpm for 10 minutes, yielding dark-coloured precipitates. These were thoroughly rinsed three times with deionized water to remove residual impurities. The cleaned precipitates were subsequently dried in an oven at 50℃ for 10 hours to eliminate moisture. For structural modification, the dried material underwent calcination at two distinct temperatures: 450°C and 600°C, each for 1 hour. A visible colour shift was observed after annealing, transitioning from dark black in the as-prepared sample to greyish-white at 450°C and finally to a bright white at 600°C, as shown in Fig. 3(a)-(c).
This progressive colour change likely reflects the thermal decomposition and removal of organic components or polymeric capping agents from the nanoparticle surfaces, indicating increased purity and crystallinity of the ZnO nanoparticles. The flow chart of the entire synthesis process, along with the possible adsorption mechanism when these nanoadsorbents are used for water remediation, has been depicted in Fig. 4.
2.4) Characterization techniques:
Several sophisticated analytical characterization techniques were utilized to investigate the structural, morphological, chemical, and optical properties of the green-synthesized ZnO nanoparticles. The crystallographic structure of the synthesized ZnO samples was investigated using the X-ray diffraction (XRD) method using a Philips X’Pert diffractometer. A glass substrate was used to spread the synthesized powdered samples, which were then mounted inside the diffractometer, and the diffraction spectra were recorded over a diffraction angle (2θ) range of 10° to 80° with a step size of 0.02°. The morphology and distribution of the synthesized ZnO nanoparticles were studied using Field emission scanning electron microscopy (FESEM) (SU8010 series, Hitachi, Japan). To identify the attached functional group and chemical bonding, Fourier transform infrared spectra (FTIR) were recorded from the L1280130 FTIR spectrometer of Perkin Elmer. Additionally, the optical behavior and absorption characteristics of the samples were analyzed using UV-Visible spectroscopy (Spectra Max iD3). To determine the concentration of heavy metal ions in untreated industrial wastewater and to assess the removal efficiency of synthesized ZnO nanoparticles, inductively coupled plasma mass spectrometry (ICP-MS) was utilized. This highly sensitive technique, performed using the Agilent 7900 ICP-MS system, enables the precise quantification of trace and ultra-trace metal ions based on their mass-to-charge (m/z) ratios after ionization in an argon plasma source. In this study, the liquid samples after adsorption were collected by filtration and transferred to 10 ml sterilized tubes. Before the ICP-MS measurements, the samples were diluted with 5% nitric acid to ensure matrix compatibility and eliminate possibilities of precipitation and adsorption losses. The concentrations of metal ions were determined using ICP-MS, with calibration standards prepared in the same acid matrix to ensure accuracy.
3) Results and discussion:
3.1) Structural analysis:
Fig. 5 illustrates the X-ray diffraction (XRD) patterns of ZnO samples corresponding to three different thermal conditions: unannealed, annealed at 450℃, and annealed at 600℃. The diffraction pattern was recorded over a diffraction angle “2θ” ranging from 10° to 80°. It was observed that in each case the diffraction profiles exhibit a series of well-defined XRD peaks that match the standard pattern of the hexagonal wurtzite structure of ZnO, which is well matched with JCPDS card No. 036-1451.
Although in each case well-defined peaks of ZnO were observed, the unannealed ZnO sample showed an additional broad hump between 20°-30° diffraction angle. This hump is generally attributed to the presence of amorphous content or poor crystallinity, which may arise from residual organic precursors as well as the formation of zinc hydroxide Zn (OH)2. This represents the incomplete conversion of precursor material to ZnO through coriander-based plant extract. Thus, additional annealing is required to ensure the complete decomposition of residual organics and Zn (OH)2. Consequently, we anneal our samples at 450℃ and 600℃ temperatures. In both cases, the broad hump disappeared, and sharp, intense peaks of ZnO phase were obtained. However, in the case of 450℃ samples, two additional peaks at diffraction angles of 28.53° and 40.58° (marked as “*”) were also observed. Upon careful investigation of these peak positions, we found that they correspond to the unreacted monoclinic phase of zinc acetate hydrate, with the peak at 28.53° attributed to the (), plane and the peak at 40.58° to the () lattice planes (JCPDS card No. 033-1464). This indicates that although we have achieved a complete conversion of Zn (OH)2 to ZnO at 450℃ annealing temperatures, traces of precursor material are still detectable. Further annealing to 600℃ reduces these residual precursor signals to a negligible level, confirming the high phase purity and improved crystallinity of ZnO. Next, we perform phase analysis using X’Pert High Score software to accurately determine the various diffraction parameters such as peak positions, full width at half maxima (FWHM), d-spacing, and corresponding lattice planes. The determined diffraction parameters for the hexagonal wurtzite structure of ZnO corresponding to unannealed, annealed at 450℃, and annealed at 600℃ have been listed in Table 2.
According to the literature, the crystallite size can be determined using the Scherrer formula as
(1)
Where the “β” is full-width at half maximum of the diffraction peaks, “0.9” is a constant introduced for the shape factor, “” is the angle of diffraction, and “λ” is the X-ray wavelength. To increase the accuracy of our results, we considered three major lattice planes (100), (002), and (101) of the ZnO wurtzite structure for crystallite size and microstrain determination. Accordingly, the calculated average crystallite size of unannealed, 450℃ annealed, and 600℃ annealed ZnO powder is 37.86 nm, 32.67 nm, and 31.86 nm, respectively, which lies in the nano range. Since amorphous Zn (OH)2 is present in the unannealed samples, which transforms to crystalline ZnO upon annealing, the annealed samples undergo densification of the microstructure. Consequently, a lower crystallite size is obtained in the case of annealed samples in comparison to the unannealed samples.
To further understand the annealing effect on the lattice structure, we calculate the lattice microstrain using the relation.
(2)
Accordingly, we observed that the unannealed ZnO sample exhibits the lowest value of microstrain of , which increases as the annealing temperature is increased to 450℃ and 600℃. The calculated values of microstrain for the 450℃ and 600℃ annealed samples are, and respectively. In the case of unannealed samples, as both amorphous Zn (OH)2 and crystalline ZnO phases exist simultaneously, the induced stress in unannealed samples is decoupled by the soft amorphous phase. However, upon annealing, the Zn (OH)2 transforms completely to the crystalline ZnO, making the lattice more rigid and continuous. Accordingly, the induced stresses can transmit across the grain boundaries. In addition to that, annealing to higher temperatures leads to the formation of various defects such as oxygen vacancies, zinc vacancies, and interstitial defects. Thus, the formation of a continuous rigid lattice and the redistribution of the defect density collectively led to an increase in the microstrain values.
Next, we determine the lattice parameters and lattice volume for a hexagonal ZnO phase by implementing the standard d-spacing equation of the hexagonal lattice as
(3)
Consequently, the lattice volume of the lattice is determined by
(4)
Where “h”, “k”, and “l” are the Miller indices of the lattice planes, “d” represents the interplanar spacing”, and “a”, “c” are the lattice constants. To calculate lattice constants, lattice planes (100), (002) and (101) planes are considered. The values obtained for “a”, “c”, “c/a” ratio, and lattice volume are tabulated in Table 3.
The obtained results suggest small changes in the structural properties of the synthesized samples with the annealing treatment. The “c/a” ratio and lattice volume of unannealed ZnO samples are 1.6017 and 47.82 (Å)3, respectively. With further annealing to 450℃ and 600℃, both “c/a” ratio and lattice volume reduce marginally to 1.6008, 1.6010, 47.79 (Å)3, and 47.67 (Å)3, respectively. This small lowering of the “c/a” ratio and lattice volume appears because of the densification of the ZnO crystalline lattice when Zn (OH)2 gets converted to crystalline ZnO upon annealing. This densification manifests as a reduction in the “c/a” ratio and a decrease in the unit-cell volume.
3.2) Morphological analysis:
Fig. 6 (a)-(c) represent the FESEM images of unannealed, 450℃, and 600℃ annealed ZnO samples, respectively, captured at a magnification of 50,000x, 1,00,000x, and 1,00,000x. Image analysis was performed using ImageJ software to estimate the average particle size, and the corresponding particle size distribution histograms with fitted normal distributions are presented alongside each image. Morphologically, all samples showed different kinds of morphology. The micrograph of the unannealed sample shows the presence of large, irregular, and agglomerated particles with an average size of about 374.66 nm. These agglomerates are distributed over relatively large distances, producing a non-uniform microstructure. The obtained morphology is consistent with incomplete crystallization and the coexistence of both crystalline ZnO and an amorphous Zn (OH)2 phase. The amorphous Zn (OH)2 component acts as a binding matrix, holding the primary ZnO crystallites together and promoting the formation of large secondary agglomerates. The presence of residual hydroxyl groups further enhances interparticle hydrogen bonding, which prevents proper dispersion and leads to clustering. As a result, the particles appear bulky and loosely packed. At 450℃, as complete crystallization has been obtained, the morphology of the particles changed, and a uniform distribution of the ZnO nanoparticles with an average particle size of 70.62 nm is obtained. However, the shape of particles is irregular, and a lower level of agglomeration can still be observed. At 600℃, the morphology of the ZnO nanoparticles becomes even more refined, and rectangular-shaped particles with an average particle size of 85.60 nm are observed.
It is noted that the crystallite size determined by the XRD analysis for 450℃ (32.67 nm) and 600℃ (31.86 nm) annealed samples is relatively lower than the estimated particle size observed in FESEM images. This difference arises because in the case of XRD, the calculated crystallite size represents the size of coherently diffracting crystalline domains, whereas FESEM reveals the physical particle size, which may consist of multiple crystallites. The larger particle size observed in FESEM is attributed to particle agglomeration and intergrowth, which are common in metal oxide nanomaterials due to their high surface energy and strong van der Waals interactions. Such agglomeration leads to the formation of secondary particles composed of several smaller crystallites, thereby resulting in larger apparent particle sizes in FESEM.
Next, we determine the elemental composition of the samples using energy dispersive spectroscopy (EDS) measurements. The EDS analysis of the ZnO samples at different annealing stages further confirms the phase evolution and compositional changes. The elemental profile of the synthesized ZnO nanoparticles has been depicted in Fig. 7 (a)-(c).
In the unannealed sample, a very high carbon content (54.5%) along with low “Zn” (9.4%) and “O” (36.1 %) is observed. The reduced “Zn” content at this stage can be attributed to the incomplete decomposition of the precursor. The hydroxide and organic species not only contribute strongly to the carbon and oxygen signals but also dilute the “Zn” signal in EDS, since “Zn” is not yet uniformly incorporated into the crystalline oxide phase. At 450℃, the Zn content increases sharply to 28.1%, while carbon decreases to 32.2%. This indicates the thermal decomposition of hydroxide and carbonaceous residues in the form of H2O and CO2, thereby reducing the carbon signal and enhancing the sample in the “Zn” signal in EDS. The higher Zn percentage reflects the more complete incorporation of Zn into the crystalline oxide lattice after the removal of non-oxide phases. Lastly, at 600℃, the Zn percentage increases slightly to 30.7%, and carbon shows a marginal decrease to 28.8%. Oxygen remains stable at nearly 40%, consistent with a predominantly ZnO lattice framework.
3.3) Optical analysis:
Fig. 8 (a) represents the absorption spectra of unannealed, 450℃, and 600℃ annealed ZnO nanoparticles.
The UV-Vis spectra show no distinct absorption edge or peak for the unannealed sample, which we attribute to its mixed-phase nature (crystalline ZnO + amorphous Zn (OH)2) and high carbonaceous residue, leading to strong light scattering that masks the ZnO band-edge transition. After annealing, well-defined ZnO absorption peaks emerge at 362.46 nm and 366.07 nm for 450℃ and 600℃ annealed samples, which are consistent with the near-band-edge transition of ZnO. To determine the optical band gap, we adopt the standard Tauc’s method in which the absorption coefficient and optical band gap are related as
(5)
Where “A” is a constant, “Eg” represents the optical band gap, represents the absorption coefficient, and the exponent “n” can have values such as 0.5, 1.5, 2, or 3 based upon the type of electronic transitions. For direct optical band gap transitions, like in ZnO, the value of exponent “n” is considered to be equal to 0.5. Thus, using the linear fitting of the 2 vs. hν plots, the optical band gap for 450℃ annealed ZnO nanoparticles and 600℃ annealed ZnO nanoparticles is estimated to be around 3.10 eV and 3.13 eV, respectively.
3.4) Chemical analysis:
To identify the chemical structure of synthesized samples, FTIR measurements are performed, and the corresponding spectra of unannealed, 450℃, and 600℃ annealed samples have been depicted in Fig. 9.
The broad peak appearing at 3248.14 cm-1 in the case of the unannealed sample corresponds to the stretching vibrations of the aromatic C-H bond. The origin of this peak is related to the presence of various phytochemicals present in the used plant extract, such as phenolic or flavonoid compounds. The noisy absorption features appearing in the spectra from 2000 cm-1 to 2500 cm-1 are primarily attributed to the interference of atmospheric CO2, and the overlap of the low-intensity absorption signal of complex constituents of the used plant extract. This makes the precise assignment of functional groups challenging. The Carboxylate (COO-) group peaks corresponding to its symmetric and asymmetric stretching mode vibrations are located at 1408.94 cm-1 and 1554.82 cm-1, respectively. This confirms the presence of residual precursor material. Further, small absorption signals corresponding to 933.08 cm-1 and 1023.06 cm-1 are attributed to the C-O-H bending and C-O stretching vibrations of flavonoid-type compounds and polysaccharides of coriander-based plant extract.
The absorption peaks in the range of 400 cm-1 to 700 cm-1 belong to the zinc intermetallic compounds. The peak at 671.06 cm-1 corresponds to the vibrational modes of the Zn-OH bond, while a small peak at 612.62 cm-1 belongs to Zn-OH bond deformation of the surface-bound species. Lastly, a weak signal of Zn-O stretching mode vibration is obtained at 458.29 cm-1. Thus, the FTIR analysis of unannealed samples showed the presence of mixed ZnO and Zn (OH)2 mixed phase, along with the presence of various plant-based phytochemicals. Further annealing the samples to 450℃ and 600℃ leads to the smoothening of the absorption spectra, indicating the breakage of loosely bonded organic species and complete decomposition of residual precursor materials. In both cases, a strong absorption peak of Zn-O lattice vibration at 458.29 cm-1 is observed. In these samples, the low intensity asymmetric stretching vibration peak of COO- group at 1554.82 cm-1 persists, but the symmetric vibration peak at 1408.94 cm-1 has completely disappeared. Further, the broad absorption centred at 3505.62 cm-1 is assigned to hydrogen-bonded O–H stretching from surface hydroxyls.
3.5) Water purification:
The batch mode adsorption method, in which the nanoadsorbents are dispersed into the solution, is adopted to purify the collected industrial wastewater from toxic elements (“Cr” and “Pb”). Four separate sets, each containing 10 mg, 20 mg, 30 mg, and 40 mg of the prepared ZnO nanoadsorbents (samples annealed at 450℃ and 600℃), are dispersed in 10 mL of industrial wastewater. Each set is then vigorously stirred for 6 hours in a dark room to achieve adsorption-desorption equilibrium. Each set was then filtered using Whatman filter paper, and then the nanoadsorbents were separated from the wastewater by centrifuging the solutions at 6,000 rpm for 10 minutes. The pH of the industrial wastewater was measured using a calibrated pH meter and was found to be approximately 6.8. Importantly, no significant change in pH was observed after the adsorption process, indicating that heavy metal ion removal did not alter the overall acidity of the wastewater. The purified wastewater samples were then characterized by inductively coupled plasma mass spectroscopy (ICP-MS) to determine the ionic concentrations of the Cr” and “Pb” in the wastewater samples. The measured ionic concentrations of “Cr” and “Pb” ions for 450℃ and 600℃ annealed ZnO nanoadsorbents corresponding to various nanoadsorbent concentrations in histogram form have been represented in Fig. 10 and Fig. 11, respectively.
To mathematically quantify the obtained results, the adsorption capacity (Qe) and removal efficiency (R.E.) values for each case are evaluated as
(6)
(7)
Where “C0” and “Ce” are the initial and final metal ion concentration of Cr and Pb ions, “M” is the mass of nanoadsorbents used, and “V” is the volume of the solution. The obtained values of “
” and “R.E” for ZnO nanoadsorbents are listed in Table 4.
Accordingly, good adsorption behaviour of “Cr” and “Pb” ions is observed for both 450℃ and 600℃ annealed ZnO nanoadsorbents. When 450℃ annealed ZnO nanoadsorbents are used, a regular increase in the removal efficiency of “Pb” and “Cr” ions was observed as the ZnO nanoadsorbent concentration is increased. In comparison to the 600℃ annealed ZnO nanoadsorbents, the 450℃ annealed ZnO nanoadsorbents displayed enhanced adsorption characteristics for “Cr” and “Pb” ions. Accordingly, removal efficiency values as high as 99.99% and 84.85% is observed for “Cr” and “Pb” ions when 40 mg/10 ml of 450℃ annealed ZnO nanoadsorbents were dispersed in industrial wastewater, respectively. Good adsorption behaviour was also seen for 600°C annealed dispersed ZnO nanoadsorbents; however, the maximum removal efficiency values achieved in this case were 69.85% and 77.69% only for “Cr” and “Pb” ions, respectively. Apart from removal efficiency, to understand the interaction of adsorbate ions and the adsorbent surface, adsorption capacity values for each concentration were calculated. However, the obtained values of the adsorption capacity don’t show any regular trend with the concentration of nanoadsorbents. This happens because the real-time adsorption process doesn’t follow a simple linear progression, since it involves various parameters such as surface site availability, adsorbate-adsorbate interactions, surface heterogeneity, and experimental conditions. Thus, to fully understand the adsorption process, different adsorption isotherm models are required. According to literature, the Langmuir and the Freundlich models are the two most widely applied adsorption isotherms to describe the interaction between adsorbates and adsorbents. The Langmuir model assumes monolayer adsorption on a homogeneous surface with finite and identical adsorption sites, implying no interaction between adsorbed molecules. In contrast, the Freundlich model is empirical and accounts for heterogeneous surface energies, allowing multilayer adsorption. The schematic of these models has already been illustrated in Fig. 4. Together, these models help in understanding the adsorption mechanism, surface properties, and efficiency of an adsorbent under different conditions. Accordingly, these adsorption models for our case have been discussed in sections 3.5.1, 3.5.2, and 3.5.3.
3.5.1) Langmuir adsorption isotherm model:
According to the Langmuir isotherm adsorption model, the adsorbent species has a homogeneous surface throughout and contains identical adsorption sites of the same energy. Accordingly, the adsorbate species has an equal probability of getting attached to the adsorbent species, which leads to the formation of a uniform monolayer of adsorbate species on the adsorbent surface.
The linear equation of the Langmuir model is given as
(8)
Where “Ce” is the equilibrium concentration of the adsorbate, “Qe” is the adsorption capacity, “Qmax” is the maximum adsorption capacity, and “KL” is the Langmuir isothermal constant.
Accordingly, the slope and intercept of the linear fitting of the graph between “Ce/Qe” and “Ce” provide the values of “Qmax” and “KL”. The Langmuir adsorption model fitting of “Cr” and “Pb” ions for 450℃ annealed and 600℃ annealed ZnO nanoadsorbents is presented in Fig. 12 (a)-(d).
3.5.2) Freundlich isotherm adsorption model:
The Freundlich isotherm adsorption model assumes the formation of multilayers on the adsorbent’s heterogeneous surface. In this model, the active sites are not identical and have different binding energies. The Freundlich adsorption isotherm can be represented in its linearized form by applying natural logarithms to the original equation, yielding the following relationship.
(9)
Where “n” represents the heterogeneity of the surface, “Kf” represents the Freundlich adsorption constant, “Ce” represents the adsorbate equilibrium concentration, and “Qe” represents the adsorption capacity. Fig. 13 (a)-(d) illustrates the Freundlich linear fitting of “Pb” and “Cr” ions for 450℃ annealed and 600℃ annealed ZnO nanoadsorbents.
3.5.3 Comparison of adsorption models:
Upon carefully examining the adsorption equilibrium fitting plots of Langmuir and the Freundlich model, it is observed that the Langmuir model showed an excellent linear fit, indicating monolayer adsorption behavior on a homogeneous surface. In all the cases, the slope of the curve remains positive and “R2” values lie close to 1. The calculated various Langmuir adsorption model parameters, such as “Qmax” and “KL”, have been listed in Table 5.
Accordingly, “Qmax” for 450℃ annealed ZnO nanoadsorbents for “Cr” and “Pb” ions is 3.33 μg/g and 1.22 μg/g, respectively. On the other hand, for 600℃ annealed ZnO nanoadsorbents, “Qmax” for “Cr” and “Pb” ions is 1.46 μg/g and 4.36 μg/g, respectively. Although in all cases we have obtained an excellent linear fit with positive “Qmax” values, in most of the cases (except for “Pb” ions adsorption in 600℃ annealed ZnO nanoadsorbents), the obtained value of “KL” is negative due to the obtained negative intercept in the linearized plot. Usually, this happens when the concentration of the adsorbate ion is very low, which is true in our case also, as the heavy metal ion concentrations in industrial wastewater are in ppb. Thus, in those cases, the value of “KL” has no physical significance. Nevertheless, for “Pb” ions adsorption in 600℃ annealed ZnO nanoadsorbents, the intercept is positive, and “KL” has a large positive value of 1140.28 L/mg. Thus, despite a few negative “KL” values, high “R2” values, and a positive Langmuir slope along with positive “Qmax” values, the Langmuir adsorption model can reasonably describe the adsorption mechanism under the extremely low concentration data set. However, complementary analysis using the Freundlich model is also necessary for a complete evaluation.
To further confirm the applicability of the Langmuir model, the equilibrium data were also fitted to the Freundlich isotherm. However, in contrast, the Freundlich model yielded negative values of “n” for all Freundlich fitted plots, along with very low and, in some cases, even negative R2 values, as listed in Table 5. A negative “n” value in the Freundlich model is physically meaningless, since in the Freundlich equation, “n” represents the heterogeneity factor or adsorption intensity, and it must be positive for favorable adsorption. When “n” lies below 1, the adsorption is favourable, and as “n” increases, the adsorption becomes less favourable. However, a negative “n” value implies that the amount adsorbed decreases with increasing equilibrium concentration, which is contrary to the fundamental behavior of adsorption. Therefore, the occurrence of negative “n” and poor correlation coefficients clearly indicates that the Freundlich model does not apply to the present system. Consequently, the Langmuir isotherm remains the most scientifically consistent and appropriate model to describe the adsorption process in this study.
In summary, the adsorption isotherm analysis indicates that model applicability is strongly influenced by experimental constraints associated with ppb-level concentrations and limited equilibrium data points. Under these conditions, physically unrealistic parameters obtained from the Freundlich model limit its mechanistic relevance. Although certain Langmuir parameters also show limitations, the Langmuir model provides a comparatively more consistent empirical description of the adsorption behavior within the scope of the present study. Accordingly, isotherm results are interpreted qualitatively rather than as definitive mechanistic proof.
4. Conclusions:
Remediation of “Pb” and “Cr” heavy metal ions from the industrial wastewater through ZnO nanoparticles adsorption was demonstrated. The ZnO nanoparticles were synthesized using a green synthesis approach in which leaves of the Coriandrum Sativum were utilized as plant extract. The as-synthesized samples showed a mixed phase of amorphous Zn (OH)2 and crystalline hexagonal wurtzite ZnO structure. Upon annealing to higher temperatures, the amorphous phase disappears, and the crystallinity improves. Further, a significant colour change from brown to white is also noted after annealing at a higher temperature. Large clusters of ZnO nanoparticles separated over large distances are observed for as-synthesized samples, while the morphology significantly improved through annealing, in which the morphology becomes more uniform and well distributed. The average particle size obtained for 450℃ and 600℃ annealed samples is 70.62 nm and 85.60 nm, respectively. Both 450℃ and 600℃ annealed ZnO nanoparticles did not show any significant change in their optical bandgap, and the measured band gap of 450℃ and 600℃ annealed ZnO is 3.10eV and 3.13 eV, respectively. Good adsorption behaviour is observed for both 450℃ annealed and 600℃ annealed ZnO nanoparticles. The 450℃ annealed ZnO nanoadsorbents showed a removal efficiency value of 84.85% for “Pb” and 99.99% for “Cr” ions for a 40mg/10ml concentration of nanoadsorbents. On the other hand, the 600℃ annealed ZnO nanoparticles showed a removal efficiency value of 77.69% for “Pb” ions using 40mg/10ml concentration of nanoadsorbents and 74.52% for “Cr” ions using 30mg/10ml concentration of nanoadsorbents. Using Langmuir and the Freundlich adsorption isotherm model, the adsorption mechanism of the heavy metal ions on ZnO nanoadsorbents is studied. The results suggest that the adsorption behaviour is better described by the Langmuir model in comparison to the Freundlich model, and the adsorption may be associated with a relatively homogeneous adsorption mechanism, in which each adsorption site is identical and has the same energy. Accordingly, our study highlights the effective and sustainable utilization of green-synthesised ZnO nanoadsorbents synthesised through Coriandrum Sativum plant extract for the remediation of heavy metal ions usually present in industrial wastewater, offering a promising route toward cleaner and safer water resources.
5) Acknowledgments:
This project is supported by the Department of Science and Technology (DST), New Delhi, India. The authors also acknowledge the sophisticated analytical instrumentation facility at Punjab University, Chandigarh, India, for helping out with XRD and FESEM measurements. The authors also acknowledge the central research facility at the Indian Institute of Technology, Delhi, India, for ICPMS measurements.
Declarations
· Ethics approval and consent to participate
We, the undersigned, declare that this manuscript is original, has not been published before, and is not currently being considered for publication elsewhere. Further, the presented work doesn’t include any experiments involving human tissues.
Signed by all authors as follows:
1) Dr. Ishan Choudhary
2) Kanika Mahajan
· Availability of data and material
The datasets generated during and/or analysed during the current study are available from the corresponding author, Dr. Ishan Choudhary, on reasonable request.
· Competing interests
We wish to confirm that there are no known conflicts of interest associated with this publication, and there has been no significant financial support for this work that could have influenced its outcome.
Signed by all authors as follows:
1) Dr. Ishan Choudhary
2) Kanika Mahajan
· Funding
The authors did not receive any specific grant from funding agencies in the public, commercial, or not-for-profit sectors.
· Author contributions
Dr. Ishan Choudhary: Experiments, original draft writing, conceptualization, validation, and supervision.
Kanika Mahajan: Experiments, characterization, methodology, data curation, and editing.
AI Statement
The authors confirm that no AI tools or services were used during the preparation of this work.