Journal of Water and Environmental Nanotechnology

Journal of Water and Environmental Nanotechnology

Photocatalytic Degradation and Adsorption Kinetics of Microwave-Assisted Bio-Synthesized ZnO Nanoflakes for Removal of Toxic Organic Pollutants

Document Type : Original Research Paper

Authors
1 School of Basic & Applied Sciences, Department of Physics, Shri Guru Ram Rai University, Dehradun-248001, Uttarakhand, India
2 School of Basic & Applied Sciences, Department of Physics, Shri Guru Ram Rai University, Dehradun-248001, Uttarakhand, India
3 Department of Physics, School of Applied & Life Sciences, Uttaranchal University, Dehradun-248007, Uttarakhand, India
4 Department of Physics, Graphic Era Deemed to be University, Dehradun-248002, Uttarakhand, India
5 SGT University, Gurugram- 122505, Haryana, India
Abstract
Zinc oxide nanoflakes (ZnO NFs) have been synthesized using a rapid and eco-friendly microwave-assisted method (400 W, 180 s) with Litchi chinensis fruit extract as a green stabilizing agent. This approach enabled the precise formation of faceted nanostructures through accelerated nucleation and growth. The structural and compositional integrity of the ZnO NFs has been confirmed by X-ray diffraction (XRD), Raman spectroscopy, Fourier-transform infrared spectroscopy (FTIR), UV–visible spectroscopy, and field emission scanning electron microscopy coupled with energy-dispersive X-ray spectroscopy (SEM–EDX). Morphological analysis verified the plate-like ZnO nanostructures. The photocatalytic and adsorption properties of the NFs have been systematically investigated against organic dyes, including Safranin O, Bromophenol Blue, and Methyl Red. The nanoflakes exhibited remarkable photocatalytic efficiency, achieving 97.36% degradation of Safranin O under UV light (125 W) within 30 min, along with strong adsorption capacity. Kinetic and isotherm studies revealed that the adsorption followed a pseudo-first-order model, with the Freundlich model indicating a maximum adsorption capacity of 541 mg/g. Furthermore, ZnO NFs demonstrated excellent recyclability over three cycles and retained high performance under varying pH and temperature conditions. These rapidly synthesized faceted nanoflakes present a promising material for photocatalytic and adsorption-based remediation of aqueous pollutants.

Graphical Abstract

Photocatalytic Degradation and Adsorption Kinetics of Microwave-Assisted Bio-Synthesized ZnO Nanoflakes for Removal of Toxic Organic Pollutants

Highlights

  • ZnO nanoflakes (NFs) prepared within 180 seconds by microwave-assisted method using Litchi chinensis pulp extract.
  • ZnO NFs shows 97.36% degradation of Safranin dye within 30 min under UV light.
  • ZnO NFs exhibits adsorption studies a high capacity of 541 mg/g for Safranin.

Keywords

1. Introduction
Untreated industrial wastewater is being released into aquatic ecosystems, and the depletion of safe water resources has become a major environmental and public health concern. [1]. The textile industry is one of the main contributors because of its extensive use of synthetic dyes, particularly azo dyes, which make up 60-70% of the 700,000 tons of textile dyes produced each year. Because they are made from aromatic hydrocarbons like toluene, benzene, aniline, phenol, and naphthalene, common azo dyes like Direct Red 28, Acid Orange 7, and Reactive Black 5 are incredibly robust and resistant to natural deterioration [2]. About 15–50% of these dyes are discharged into wastewater streams as a result of inefficient dyeing processes, which significantly raises the chemical and biological oxygen demands (COD and BOD) value ranges from 1000-3000 mg/L (COD) and 200-700 mg/L (BOD), which are well above the safe discharge upto 50 mg/L and 10 mg/L, respectively [3-5]. These colors also change the physicochemical qualities of water, elevating pH levels (between 10 and 11) and adding substantial inorganic content, which harms aquatic ecosystems [6]. Azo dyes are highly resistant to standard water treatment technologies due to their complicated structures, which include azo bonds (-N=N-) and aromatic rings. This persistence underlines the critical need for innovative and effective removal technologies that can reduce their toxicity, bioaccumulation, and long-term environmental impact [7-9]. Water pollution continues to be one of the most urgent worldwide issues among various environmental issues, requiring the creation of efficient wastewater treatment technology [10]. Numerous treatment techniques, such as adsorption, photocatalysis, co-precipitation, and biological processes, have been studied to eliminate contaminants from industrial effluents. Adsorption and Photocatalysis are two of the most effective and environmentally friendly color removal processes. Metal oxide nanoparticles (NPs) such as CdS, ZnO, Ag, Au, TiO₂, and SnO₂, are now widely used in wastewater treatment [11-14]. Among these, zinc oxide (ZnO) has emerged as a highly adaptable material due to its wide bandgap of around 3.37 eV. Its low toxicity, ease of synthesis, and cost-effectiveness make it a popular choice for a variety of applications. ZnO has been intensively explored for usage in photocatalysis, solar energy harvesting, UV lasers, and sensor technologies, demonstrating its broad scientific and industrial applications [15-17]. Notably, multiple studies have confirmed ZnO nanoparticles’ effective photocatalytic activity, making them a suitable alternative for wastewater treatment and other environmental remediation initiatives. For example, Mahajan et al. used Justicia adhatoda (J. adhatoda) extract of leaf to synthesize zinc oxide nanoparticles (ZnO NPs) with the smallest crystallite and particle diameters reported to date, 5.2 nm and 12.41 nm, respectively. The resultant ZnO NPs displayed excellent photocatalytic efficiency, degrading Malachite Green (MG) dye by 99.8% in 180 min [18]. Similarly, Kaur et al. used Elettaria cardamomum pod (EC-pod) extract for green production of ZnO NPs as a sustainable method of environmental cleanup. The generated ZnO NPs demonstrated outstanding photocatalytic activity, degrading MG dye by 99.8% under UV irradiation in 160 min [19]. Jamil et al. use H2O2 as a reduction agent for the production of ZnO NPs, and Violet 26 dye is degraded. It has been found that the DE of 93% in 60 min under UV irradiation [20]. Seyed Masoud et al. synthesized nanoparticles supported on multi-walled carbon nanotubes of ZnO for the removal of Congo red dye, which shows DE~99.8% in 120 min [21]. Sauvik et al. synthesized CuO/Mn3O4/ZnO NCs for the removal of Rabeprazole from water, which shows 84.45% of total removal in 60 min [22]. Manaswini et al. utilized Tabernaemontana divaricata green leaf extract to produce zinc oxide nanoparticles (ZnO NPs) and experimentally found out their biosorptive properties. The study reported a maximum Congo Red (CR) dye removal efficiency of 93.1%. [23]. Asad et al. synthesized CeO2-ZnO NCs for the removal of MB dye, which showed DE~92% in 210 min [24]. Similarly to this, Basnet et al. destroyed RhB dye while synthesizing ZnO NPs using glycine as a reducing agent. It has been discovered that 15 min of UV exposure is sufficient to obtain a DE of 80% [25]. Sarita et al. have synthesized ZnO nanocomposites (NCs) to remove Cd2+ ions in aqueous solutions, and show the max adsorption capacity (MAC) of 96.15 mg/g for Cd2+ ions [26]. K Saini et al. have synthesised ZnO platelets by Asoka Leaves against the adsorption of MG dye, which shows a maximal adsorption capacity of 331 mg/g [27]. T Budhiraja et al. synthesised activated carbon from oak wood against the adsorption of MB dye, and the result shows MAC 40.98mg/g [28]. Although numerous methods exist for synthesizing ZnO nanostructures (NSs), conventional techniques often involve harsh chemicals that can leave toxic residues on the ZnO surface, limiting their applicability in sensitive areas such as biomedical and environmental systems. This gap has driven the exploration of greener, more sustainable synthesis strategies. Among them, plant-mediated approaches have emerged as a novel and effective alternative, offering eco-friendly, residue-free, and biocompatible ZnO NSs. Such green routes not only address safety concerns but also provide additional advantages, including cost-effectiveness, rapid synthesis, and the potential to tailor surface functionalities through natural phytochemicals, thereby expanding the scope of ZnO applications in biomedical, environmental, and catalytic fields [29]. Microwave-assisted synthesis has emerged as a promising alternative due to its ability to enable rapid, controlled nucleation and growth of nanostructures with significantly lower energy consumption than conventional methods. However, the synthesis of faceted ZnO NSs using plant extracts via this approach remains largely unexplored. 
In this study, ZnO nanoflakes (NFs) have been rapidly synthesized through microwave irradiation (400 W, 180 s) employing Litchi chinensis (Lychee) fruit extract as a green reducing agent. The resulting multidimensional ZnO NFs were systematically characterized and evaluated for their photocatalytic and adsorption performance toward various dyes under both UV and visible light.
 
2. Materials and Methods
2.1 Materials
Zinc sulfate hexahydrate (ZnSO4·6H2O, 96% purity) and sodium hydroxide (NaOH, 98% purity) were obtained from Central Drug House Pvt. Ltd., located in Delhi, India. Litchi chinensis fruits, acquired from a nearby market, served as a green medium for the synthesis of ZnO NFs. Safranin (chemical structure: C20H19ClN4, molar mass: 350.84 g/mol, and ƛmax: 519 nm), Bromophenol Blue (chemical structure: C₁₉H₁₀Br₄O₅S, molar mass: 669.96 g/mol, and ƛmax: 590 nm), Methyl Red (chemical structure: C15H15N3O, molar mass: 269.304 g/mol, and ƛmax: 430 nm), as shown in Fig. 1(a), with a purity of 99.9% supplied by Central Drug House Pvt. Ltd. (Delhi, India). Double-distilled water (DW) was utilized throughout the procedure to guarantee high purity.
 
2.2 Preparation of ZnO NFs
Litchi chinensis fruit extract served as a green medium for the synthesis of ZnO NFs. Fresh Litchi chinensis fruits were gathered, thoroughly washed, and shade-dried for a period of 15 days. The dried fruit pulp was finely ground, and 10 g of it was combined with 100 ml of deionized water (DW), then heated to 70°C for 1 hour. The mixture was filtered through Whatman filter paper (Grade 42), and the resulting filtrate, referred to as LCPx, was stored in a refrigerator for future use. Subsequently, 1M ZnSO4·6H2O was introduced to 100 ml of LCPx, and the pH was adjusted to approximately 9 using NaOH pellets. The solution was stirred and sonicated for 15 min. Following this, the mixture was subjected to microwave treatment (IFB, 20PM-MEC2) at 40% power (~400W) for 3 min. The resultant product was washed, filtered, and dried at 80°C for 12 hours under ambient conditions. Ultimately, the product was calcined at 300 °C in a muffle furnace for 3 hours to eliminate biological impurities, resulting in a whitish ZnO NFs powder suitable for further applications.
 
2.3 Photocatalytic activity
The efficiency of photocatalytic degradation for Safranin, Bromophenol Blue (BB), and Methyl Red (MR) was assessed under both visible and UV irradiation (125 W). A specially designed photocatalytic reactor (dimensions: 30 × 30 × 45 cm³, working distance: 12 cm) was utilized, which included a light source. Visible (white) light was generated using a 125 W high-pressure mercury vapor (HPMV) bulb that was coated with phosphor, while UV light was produced by the same type of bulb but without the phosphor coating. To evaluate the photocatalytic degradation potential of ZnO NFs, 100 ml of dye solution (1 mg/l) was combined with 0.1 mg/ml of ZnO NFs in a 250 ml beaker. This mixture was subsequently exposed to either UV or visible light within the reactor, with continuous stirring facilitated by a magnetic stirrer. Samples were taken at specified time intervals, and the dye concentration was measured using the Beer-Lambert law. The dye degradation efficiency (DE%) was computed using the following formula: 
(DE)% = (C₀ - Ct) / C₀ * 100
where C₀ represents the initial concentration of dye, and Ct is the concentration at time t, demonstrating the photocatalytic efficiency of ZnO NFs.
 
2.4 Adsorption experiments
The synthesized ZnO NFs were assessed for their adsorption capabilities utilizing Safranin dye (initial concentration, C0 = 1 mg/L). The procedure involved combining 100 mL of the dye solution with 0.01 g of ZnO NFs in a flask. The mixture was stirred at 160 rpm on a magnetic stirrer for a duration of 60 min. Samples were taken every 10 min to observe the progress of dye adsorption. The concentration of dye in each sample was measured using a UV-Vis spectrophotometer. The dye removal efficiency (RE) and adsorption capacity (qe) of the ZnO NFs were computed using Equations 1 and 2, respectively.
RE(%), h = (C0 –Ce)/C0 x 100      (1) 
qe = (C0 – Ce) x V/M      (2)
Where C0 is the initial concentration of dye, Ce ​ is the equilibrium concentration of dye, qe ​ (mg/g) is the equilibrium adsorption capacity, V (L) is the volume of the solution of dye , and M (g) is the mass of ZnO NFs used in Equations 1 and 2
 
2.5. Adsorption kinetics
The linear equations of the pseudo-first-order (Eq. 3) and pseudo-second-order (Eq. 4) kinetic models were utilized to examine the adsorption mechanism [30].
 Where qe(mg/g) represents the quantity of dye adsorbed at equilibrium, qt(mg/g) denotes the quantity of dye adsorbed at time t (min), k1 (min-1) signifies the pseudo-first-order rate constant, and k2 (g/mg.min) indicates the pseudo-second-order rate constant.
 
2.6. Adsorption Isotherm
The adsorption characteristics of Safranin onto ZnO NFs were examined utilizing the Langmuir (Eq. 5) and the Freundlich (Eq. 6) isotherm models [31,32]. The Langmuir isotherm posits that adsorption occurs in a monolayer on a uniform surface with consistent adsorption energies [31], while the Freundlich model considers adsorption on a non-uniform surface with varying energy distribution and the potential for multilayer adsorption [32]. Studies 
 
Adsorption isotherms were conducted by altering the initial concentration of Safranin dye from 1 to 10 mg/L.
 
In Equations 5 and 6, Ce (mg/L) signifies the equilibrium dye concentration, qe (mg/g) indicates the equilibrium adsorption capacity, qmax (mg/g) refers to the maximum monolayer adsorption capacity, KL (L/mg) represents the Langmuir isotherm constant associated with adsorption energy, KF (mg/g) is the Freundlich affinity coefficient, and 1/n is the Freundlich linearity constant that reflects the intensity of adsorption. A schematic illustration of the synthesis procedure for ZnO NFs and the subsequent evaluation of their photocatalytic activity and adsorption capabilities is provided in Fig. 1(b).
 
2.4 Characterization
The structural analysis of the synthesized ZnO NFs was conducted utilizing X-ray diffraction (XRD) with a PANalytical X’Pert Powder diffractometer that is equipped with a Cu Kα radiation source. Raman spectra were obtained using a LabRam HR 800 UV Micro-Raman spectrometer (Jobin-Yvon) with a He-Ne laser excitation source operating at a wavelength of 633 nm. Fourier Transform Infrared Spectroscopy (FTIR) analysis was carried out using a Bruker TENSOR 27 instrument across the range of 4000–400 cm⁻¹, with samples prepared in the form of KBr pellets. The surface morphology of the ZnO NFs was characterized through Field Emission Scanning Electron Microscopy (FESEM) employing a JEOL JSM-7100F. The optical absorption properties were examined using a UV-vis spectrophotometer (Perkin Elmer Lambda 1050). Photocatalytic and adsorption activities were assessed based on absorbance measurements taken with the PerkinElmer Lambda 650 UV-vis spectrophotometer, and dye concentrations were calculated using the Beer–Lambert law.
 
3. Results and Discussions
3.1 Structural Analysis
Fig. 2(a) illustrates the X-ray diffraction (XRD) pattern of the synthesized ZnO NFs. A significant diffraction peak is noted at 2θ ≈ 33.85°, which is associated with the (100) crystal plane. Additional peaks can be seen at 35.37° (002), 37.68° (101), 42.05° (102), 51.55° (103), 58.61° (200), 60.38° (112), and 62.9° (201). These peaks are in good agreement with the standard data from the JCPDS card no. 36-1451, thereby confirming the formation of ZnO with a hexagonal wurtzite crystal structure [33]. Fig. 2(b) shows the Raman spectrum of the ZnO NFs. The detected modes correspond to the optical phonons of hexagonal wurtzite ZnO at the Γ point of the Brillouin zone, identified as A1, 2B1, E1, and 2E2 modes. [34]. The E1 and A1 polar vibrational modes of ZnO are active in both infrared and Raman spectroscopy, whereas the B1 modes are inactive in both techniques. Additionally, the A1 and E1 modes are categorized into longitudinal optical (LO) and transverse optical (TO) phonons. A notable and sharp E2 (high) mode, observed at 446 cm⁻¹, is recognized as the characteristic Raman-active nonpolar phonon mode of wurtzite ZnO, primarily linked to the displacement of oxygen atoms. A less intense peak at 445.28 cm⁻¹ may be ascribed to a multi-phonon scattering process that involves the difference between the E2 (high) and E2 (low) modes. The mode detected at 332.62 cm⁻¹ is likely attributed to the A1 (TO) vibration, while the peak at 541.31 cm⁻¹ is associated with the A1 (LO) mode. The pronounced intensity of the E2 (high) peak, in conjunction with the relatively weak E1 (LO) mode, affirms the high crystallinity and the hexagonal wurtzite structure of the synthesized ZnO NFs.
Fig. 2(c) illustrates the FTIR spectrum of ZnO NFs. The characteristic absorption band at 509.98 cm⁻¹ corresponds to Zn–O stretching vibrations, thereby confirming the successful formation of ZnO. The broad peaks observed around 883.44 cm⁻¹ are linked to Zn–OH bonds. The presence of C=O stretching vibrations is evident from the peaks located between 1396 and 1572 cm⁻¹, while the absorption band at 2924 cm⁻¹ corresponds to C–H stretching vibrations. A strong and broad absorption band at 3379 cm⁻¹ indicates the presence of O–H groups, suggesting the existence of surface-adsorbed water molecules on the ZnO nanoparticles [33]. Fig. 2(d) presents the UV–visible absorption spectrum of the ZnO NFs. The absorption edge is observed around 370 nm, indicating effective absorption in the UV region. The ZnO NFs demonstrate high transparency in the visible range, permitting most visible light to pass through, which is a distinctive characteristic of ZnO nanoparticles. Furthermore, the energy bandgap (Eg) of the synthesized ZnO NFs was estimated using the Tauc plot method (inset of Fig. 2d), resulting in an Eg value of 3.32 eV. This result is in close agreement with the typical bandgap reported for ZnO NSs.
 
3.2 Morphological Analysis
FESEM was used to investigate the surface morphology of synthesised ZnO NFs. The FESEM micrographs (Fig. 3a) show that the ZnO NFs are made up of randomly crumpled, thin plate-like nanostructures with an average thickness of around 46.73 nm. Fig. 3b Shows the EDX Spectrum of ZnO NFs. A range of factors influences the formation of such nanostructures, including parameters of microwave synthesis such as temperature, radiation energy, power, and reaction duration. Additionally, the characteristics of solvents and precursors—like solvent polarity, precursor concentration, pH, the type of reducing agent, and the existence of surface-modifying agents—play a crucial role in the development of crystallites [34-35]. In this study, LCPx acts as both a reducing and complexing agent. The interaction between ZnSO₄·6H₂O and LCPx results in the formation of Zn(OH)₂, which subsequently dissociates into Zn²⁺ and OH⁻ ions (Equation 2), facilitating the nucleation and growth of ZnO NPs (Eq. 3). [36].
 Equation 3 illustrates the direct precipitation of ZnO nuclei within the solution, which subsequently expand and merge to form nanoplatelets (NPLs) exhibiting diverse morphologies. ZnO NFs develop through the stacking of tetrahedral O²⁻ and Zn²⁺ ions along the c-axis, leading to the formation of alternating planes. Polar surfaces arise from the presence of oppositely charged ions, such as the positively charged Zn²⁺ (0001) face and the negatively charged O²⁻ face [37-38]. A similar morphology of NFs has also been documented previously [27]. This polarity induces spontaneous polarization along the c-axis, facilitating the self-catalysed development of nanostructures (NS) through electrostatic interactions. Additionally, the pH of the reaction medium plays a significant role in determining the shape of the resulting structures. It has been demonstrated that pH levels exceeding 9 encourage the formation of nanostructures with higher aspect ratios (length/diameter). Our findings demonstrate that simple, microwave-assisted approaches can effectively manufacture large, multidimensional ZnO structures, avoiding the requirement for sophisticated catalytic or surfactant-driven synthesis processes. Furthermore, the use of a highly polar solvent in this method certainly contributed to lower synthesis temperatures, lower energy consumption, and faster reaction times (180 seconds) [39]. Table S1 shows a comparative examination of distinct ZnO morphologies synthesized utilizing various fruit extracts and green synthesis methodologies.
 
3.3 Photocatalytic activity
The photocatalytic performance of the synthesized ZnO NFs was evaluated by determining their capacity to degrade Safranin, Bromophenol Blue (BB), and Methyl Red (MR) dyes at a concentration of 0.1 mg/mL, under both UV (125 W) and visible light exposure. When subjected to UV light, ZnO NFs demonstrated an impressive degradation efficiency (DE) of 97.36% for Safranin after a duration of 30 minute (Fig. 5a),. Conversely, under visible light, the DE significantly decreased to 22% with the same concentration of ZnO (Fig. 5b),. The degradation kinetics adhered to pseudo-first-order kinetics, represented by the equation: ln(C₀/Ct) = kt, where k (min⁻¹) denotes the rate constant, and C₀ and Ct signify the initial and final dye concentrations, respectively [38]. For Safranin, the rate constant k under UV irradiation was determined to be 0.010018 min⁻¹(Fig. 5d, f), whereas under visible light it was 0.00797 min⁻¹(Fig. 6c, e), confirming the enhanced activity driven by UV light. Similarly, for Bromophenol Blue, ZnO NFs (0.1 mg/mL) reached a 93% DE under UV light after 30 min (Fig. 6a), in contrast to only 33% under visible light (Fig. 6b). The calculated rate constants were 0.08501 min⁻¹ under UV (Fig. 6d, f) and 0.01061 min⁻¹ under visible light (Fig. 6c, e). Regarding Methyl Red, the ZnO NFs achieved a 95% DE under UV light within 30 min (Fig. 7a), while only 32% degradation was observed under visible light (Fig. 7b). The respective rate constants were 0.1053 min⁻¹ under UV (Fig. 7d, f) and 0.01021 min⁻¹ under visible light (Fig. 7c, e). A comparative analysis of the degradation efficiency of ZnO NSs has been tabulated in Table 1  [40-44].

3.5 Adsorption studies
The synthesized ZnO NFs were assessed for their adsorption capabilities concerning Safranin dye at various concentrations (1–10 mg/L), pH levels, and temperatures. Initially, adsorption experiments were performed at different pH values (3, 6, and 10) at ambient temperature, followed by temperature adjustments (30 , 40 , and 50 °C) while maintaining a constant pH of approximately 6. For the isotherm study, ZnO NFs (0.1 mg/mL) were introduced into 100 mL of Safranin dye solutions with varying concentrations (1–10 mg/L). The mixtures were agitated at 160 rpm for 60 min using a magnetic stirrer, and samples were taken every 10 min. The removal efficiency (RE) and adsorption kinetics are illustrated in Fig. 8(a–d). The removal efficiency was noted to decline with increasing dye concentration: 83%, 52%, 28%, 24%, and 21% for 1, 3, 5, 7, and 10 mg/L, respectively. A similar pattern was observed with rising temperature, where RE decreased to 83%, 43%, and 29% at 30 °C, 40 °C, and 50 °C, respectively. In contrast, variations in pH had a notable impact, with RE values of 83%, 55%, and 85% at pH 6, 3, and 9, respectively (Fig. 9a–d). The endothermic nature of the adsorption process was validated by the reduced efficiency at elevated temperatures, likely due to diminished diffusion rates of Safranin dye and a decrease in available active sites on the ZnO surface. At higher temperatures, thermal agitation may lead to the desorption of previously adsorbed dye molecules, thereby lowering overall efficiency [35]. Conversely, the adsorption performance was enhanced at higher pH levels. This improvement can be attributed to electrostatic interactions: Safranin (a cationic dye, 3,7-dimethyl-10-phenylphenazin-10-ium-2,8-diamine chloride) interacts favorably with the negatively charged surface of ZnO NFs at elevated pH, promoting dye uptake. The adsorption mechanism is primarily influenced by electrostatic interactions and functional groups such as carboxyl, amino, and hydroxyl groups, which facilitate bonding between the dye and the ZnO surface [45]. The adsorption data were analysed using kinetic models, specifically, pseudo-first-order and pseudo-second-order, as illustrated in Fig. 9c–d. The findings indicated that the pseudo-first-order model yielded a more accurate representation of the experimental data. For isotherm modelling, both the Langmuir and the Freundlich models were utilized (refer to Fig. S2, Table 2). The Freundlich model demonstrated a marginally better fit, suggesting the occurrence of multilayer adsorption behaviour. The maximum capacity for dye adsorption was determined to be 541 mg/g, based on the Freundlich isotherm model. On the other hand, the pHpzc value of ZnO NFs is obtained as ~8.71 (SI, S1, Fig. S3). At pH values below 8.71, the ZnO surface carries a positive charge, which causes electrostatic repulsion with the cationic dye Safranin and results in relatively lower adsorption. In contrast, at pH values above 8.71, the ZnO surface becomes negatively charged, favouring strong electrostatic attraction with Safranin molecules and thereby enhancing adsorption and removal efficiency. The adsorption behaviour observed in our study aligns well with this surface charge mechanism, confirming the experimentally determined pHpzc value of 8.71 for ZnO NFs. A comparative analysis presented in Table 3 showcases ZnO-based structures, emphasizing the enhanced dye removal efficiency of the synthesized ZnO nanofibers. It is evident from the results that the synthesized ZnO NFs exhibit remarkable photocatalytic performance, achieving 97.36% degradation of Safranin under UV light within 30 min, along with a high adsorption capacity of 541 mg/g, surpassing many conventional ZnO NSs. The study further demonstrates the material’s stability, reusability, and effectiveness across a range of pH and temperature conditions. These findings highlight the material’s high functional efficiency, environmental safety, and potential applicability in both environmental and biomedical domains, offering valuable insights for nanomaterial design and pollutant remediation.
 
3.6 Reusability of ZnO NFs 
The recyclability of ZnO NFs was evaluated by examining their photocatalytic and adsorption capabilities for Safranin dye across several usage cycles, as depicted in Fig. 10. In each cycle, a 100 mL solution of 1 mg/L Safranin was treated with 0.1 mg/mL ZnO NFs in a flask. Following treatment, the ZnO NFs were separated through filtration, and the concentration of residual dye in the solution was monitored to assess removal efficiency. The recovered ZnO NFs were thoroughly washed with water, dried at 70 °C, and reused in two additional cycles (Cycles 2 and 3). The results demonstrated that ZnO NFs retained their activity for up to three cycles, although a gradual decline in efficiency was observed. Photocatalytic degradation efficiency (DE) decreased from 97.36% in Cycle 1 to 24% in Cycle 3 (Fig. 10ab), while the adsorption removal efficiency (RE) dropped from 83% to 33% over the same cycles (Fig. 10cd). These results confirm that while ZnO NPs exhibit good initial activity, their performance diminishes over repeated use due to potential surface fouling or structural degradation.
3.7 Dye removal mechanisms of ZnO NFs
Our experimental results indicate that Safranin dye removal by ZnO NFs proceeds via two primary mechanisms: adsorption and photocatalytic degradation (Fig. 11). In the absence of light, dye removal is solely governed by physical adsorption, which may occur as monolayer or multilayer adsorption driven primarily by electrostatic interactions between ZnO NFs and dye molecules (Fig. 11b). This adsorption mechanism is affected by a variety of interactions, such as electrostatic attraction, ion exchange, Van der Waals forces, hydrogen bonding, and π–π stacking. These interactions frequently occur simultaneously, with the overall process being influenced by the molecular structure of the dye, the pH of the solution, and the surface properties of ZnO NFs (Fig. 3a). FTIR analysis (Fig. 2c) further indicates the participation of functional groups like hydroxyl, amino, and carboxyl groups, which are crucial in determining the adsorption behavior. The second mechanism involves photocatalysis, which is triggered by exposure to UV or visible light. When ZnO NFs absorb photons with energy that meets or exceeds their bandgap (~3.32 eV), electrons are excited from the valence band to the conduction band, resulting in the formation of corresponding holes. These photo-induced electron–hole pairs migrate to the surface of the catalyst, where they initiate redox reactions. The excited electrons react with oxygen molecules to form superoxide radicals (•O₂⁻), while the holes can interact with hydroxide ions (OH⁻) or water molecules to generate hydroxyl radicals (•OH). Both types of radicals are highly reactive and play a significant role in the oxidative degradation of Safranin dye molecules. The presence of UV light enhances this process by producing a greater number of electron–hole pairs, thus increasing the photocatalytic efficiency. Consequently, under UV irradiation, the degradation of the dye is considerably more effective due to the synergistic action of these reactive species (Fig. 11a). The reduction mechanism of Safranin can be described by Eqs. 4-7  [38].
ZnO + hʋ→    ZnO (e− + h+)  (4)
H+ + •O2- → •OH  (5)
h+ + H2O → H+ + •OH (6)
h+ + •O2-  + •OH + Safranin → CO2+H2O (7)
 
4. Conclusion 
In this research, a green, rapid, and straightforward microwave-assisted synthesis technique (400 W, 180 seconds) was utilized to produce ZnO NFs using Litchi chinensis fruit extract as a natural reducing agent. Analysis of surface morphology confirmed the creation of plate-like nanostructures. The synthesized ZnO NFs were comprehensively examined for their photocatalytic and adsorption capabilities against organic dyes such as Safranin, BB, and MR. Under 125 W UV irradiation, the ZnO NFs exhibited exceptional photocatalytic activity, achieving a peak degradation efficiency of 97.36% for Safranin dye within 30 min. They also demonstrated significant performance under visible light. Adsorption experiments were carried out under varying conditions of temperature, pH, and dye concentration. The adsorption kinetics adhered to a pseudo-first-order model, while the isotherm data were characterized by both both the Freundlich and Langmuir models, with a MAC of 541 mg/g estimated using the Freundlich isotherm. Recyclability assessments indicated that the ZnO NFs retained substantial photocatalytic and adsorption efficiency over three consecutive cycles, demonstrating good stability and reusability. Overall, the faceted ZnO NFs synthesized through a rapid and eco-friendly microwave method show considerable potential for applications in environmental remediation, particularly in the adsorption-based removal and photocatalytic degradation of pollutants in water.
 
Acknowledgements
The authors gratefully acknowledge Sri Guru Ram Rai University for providing financial support.
 
Conflict of Interest
The authors declare no conflict of interest.
 
Funding
SGRR University provided financial support (Seed Money Project No: SGRRU/DR (11)2023 /SM01) for the project. 
 
Author’s Contributions
Study Conception or Design: VR
Data Acquisition: AC; VR
Data Analysis or Interpretation: VR; TB
Manuscript Drafting: VR; BR; SK; AKK
Critical Manuscript Revision: PC
All authors have approved the final manuscript and are responsible for all aspects of the work.
 
AI Statement
During the preparation of this work the author(s) used Grammarly and ChatGPT free version in order to check grammar and polishing the text. After using this tool/service, the author(s) reviewed and edited the content as needed and take(s) full responsibility for the content of the publication.
 
 
[1] Singh, B. J., Chakraborty, A., & Sehgal, R. (2023). A systematic review of industrial wastewater management: Evaluating challenges and enablers. Journal of Environmental Management, 348, 119230.
[2] Artifon, W., Cesca, K., de Andrade, C. J., de Souza, A. A. U., & de Oliveira, D. (2021). Dyestuffs from textile industry wastewaters: Trends and gaps in the use of bioflocculants. Process Biochemistry, 111, 181-190.
[3] Davarpanah, M., Ahmadpour, A., & Bastami, T. R. (2015). Preparation and characterization of anion exchange resin decorated with magnetite nanoparticles for removal of p-toluic acid from aqueous solution. Journal of Magnetism and Magnetic Materials, 375, 177-183.
[4] Kaur, A., Kumar, S., Kaur, H., Lotey, G. S., Singh, P. P., Singh, G., ... & Kaushal, S. (2024). Enhanced photocatalytic degradation and antimicrobial activities of biogenic Co 3 O 4 nanoparticles mediated by fenugreek: sustainable strategies. Materials Advances, 5(20), 8111-8131.
[5] Bahrami, S., Ahmadpour, A., Bastami, T. R., Ayati, A., & Mirzaei, S. (2024). Comparative study of metal nanoparticles anchored TiO2 using polyoxometalate intermediate in photodegradation of azo dye pollutant in aquatic environments. Inorganic Chemistry Communications, 160, 111986.
[6] Khan, A., Ju, P., Han, Z., & Ni, C. (2024). A comprehensive review on adsorptive removal of azo dyes using functional materials. AQUA—Water Infrastructure, Ecosystems and Society, 73(2), 266-285.
[7] Bastami, T. R., & Entezari, M. H. (2013). High stable suspension of magnetite nanoparticles in ethanol by using sono-synthesized nanomagnetite in polyol medium. Materials Research Bulletin, 48(9), 3149-3156.
[8] Rohilla, S., Gupta, A., Kumar, V., Kumari, S., Petru, M., Amor, N., ... & Dalal, J. (2021). Excellent UV-light triggered photocatalytic performance of ZnO. SiO2 nanocomposite for water pollutant compound methyl orange dye. Nanomaterials, 11(10), 2548.
[9] Twinkle, T., Saini, K., Shukla, R. K., Bezbaruah, A. N., Gupta, R., Kar, K. K., ... & Chamoli, P. (2022). Nanomaterials and Purification Techniques for Water Purification and Wastewater Treatment. In Nanomaterials for Advanced Technologies (pp. 103-125). Singapore: Springer Nature Singapore.
[10] Saravanan, A., Kumar, P. S., Jeevanantham, S., Karishma, S., Tajsabreen, B., Yaashikaa, P. R., & Reshma, B. (2021). Effective water/wastewater treatment methodologies for toxic pollutants removal: Processes and applications towards sustainable development. Chemosphere, 280, 130595.
[11] Patra, A. K., & Pariti, S. R. K. (2022). Restricted substances for textiles. Textile Progress, 54(1), 1-101.
[12] Pathania, D., Sharma, M., Kumar, S., Thakur, P., Torino, E., Janas, D., & Thakur, S. (2021). Essential oil derived biosynthesis of metallic nano-particles: Implementations above essence. Sustainable Materials and Technologies, 30, e00352.
[13] Hassabo, A. G., Zayed, M., Bakr, M., & Othman, H. (2022). An overview of carpet manufacture: Design, dyeing, printing and finishing. Journal of Textiles, Coloration and Polymer Science, 19(2), 269-290.
[14] Crini, G., Lichtfouse, E., Chanet, G., & Morin-Crini, N. (2020). Applications of hemp in textiles, paper industry, insulation and building materials, horticulture, animal nutrition, food and beverages, nutraceuticals, cosmetics and hygiene, medicine, agrochemistry, energy production and environment: A review. Environmental Chemistry Letters, 18(5), 1451-1476.
[15] An, L., Liu, Q., Deng, Y., Wu, W., Gao, Y., & Ling, W. (2020). Sources of microplastic in the environment. Microplastics in terrestrial environments: Emerging contaminants and major challenges, 143-159.
[16] Chamoli, P., Shukla, R. K., Bezbaruah, A. N., Kar, K. K., & Raina, K. K. (2021). Ferrites for Water Purification and Wastewater Treatment. Ferrites and Multiferroics: Fundamentals to Applications, 117-127.
[17] Lofrano, G., Meriç, S., Zengin, G. E., & Orhon, D. (2013). Chemical and biological treatment technologies for leather tannery chemicals and wastewaters: A review. Science of the Total Environment, 461, 265-281.
[18] Mahajan, M., Kumar, S., Gaur, J., Kaushal, S., Dalal, J., Singh, G., ... & Ahlawat, D. S. (2025). Green synthesis of ZnO nanoparticles using Justicia adhatoda for photocatalytic degradation of malachite green and reduction of 4-nitrophenol. RSC advances, 15(4), 2958-2980.
[19] Kaur, H., Sharma, A., Anand, K., Panday, A., Tagotra, S., Kakran, S., ... & Singh, G. (2025). Green synthesis of ZnO nanoparticles using E. cardamomum and zinc nitrate precursor: a dual-functional material for water purification and antibacterial applications. RSC advances, 15(21), 16742-16765.
[20] Jamil, A., Bokhari, T. H., Javed, T., Mustafa, R., Sajid, M., Noreen, S., ... & Jilani, M. I. (2020). Photocatalytic degradation of disperse dye Violet-26 using TiO2 and ZnO nanomaterials and process variable optimization. Journal of Materials Research and Technology, 9(1), 1119-1128.
[21] Arabi, S. M. S., Lalehloo, R. S., Olyai, M. R. T. B., Ali, G. A., & Sadegh, H. (2019). Removal of congo red azo dye from aqueous solution by ZnO nanoparticles loaded on multiwall carbon nanotubes. Physica E: low-dimensional systems and nanostructures, 106, 150-155.
[22] Raha, S., Mohanta, D., & Ahmaruzzaman, M. (2021). Novel CuO/Mn3O4/ZnO nanocomposite with superior photocatalytic activity for removal of Rabeprazole from water. Scientific reports, 11(1), 15187.
[23] Manaswini, K. S., Chitti Babu, N., & Bhavani, Y. (2023, December). Green Synthesis of Zinc Oxide Nanoparticles and Its Adsorptive Studies on Removal of Congo Red Dye. In Indian Chemical Engineering Congress (pp. 197-217). Singapore: Springer Nature Singapore.
[24] Syed, A., Yadav, L. S. R., Bahkali, A. H., Elgorban, A. M., Abdul Hakeem, D., & Ganganagappa, N. (2020). Effect of CeO2-ZnO nanocomposite for photocatalytic and antibacterial activities. Crystals, 10(9), 817.
[25] Basnet, P., Samanta, D., Chanu, T. I., Jha, S., & Chatterjee, S. (2020). Glycine-A bio-capping agent for the bioinspired synthesis of nano-zinc oxide photocatalyst. Journal of Materials Science: Materials in Electronics, 31, 2949-2966.
[26] Alhan, S., Nehra, M., Dilbaghi, N., Singhal, N. K., Kim, K. H., & Kumar, S. (2019). Potential use of ZnO@ activated carbon nanocomposites for the adsorptive removal of Cd2+ ions in aqueous solutions. Environmental research, 173, 411-418.
[27] Saini, K., Rawat, V., Semwal, S., Rawat, B., Kar, K. K., Raina, K. K., & Chamoli, P. (2024). Saraca asoca-assisted green synthesise of ZnO nanoplatelets for photocatalytic activity and adsorption kinetics. Int. J. Environ. Anal. Chem., 1–21., 
[28] Budhiraja, T., Rawat, V., Kimothi, S., Dumka, U. C., Gupta, R., Penke, Y. K., ... & Chamoli, P. (2024). Low temperature physical activation of raw charcoal for excellent dye adsorption kinetics. Fullerenes, Nanotubes and Carbon Nanostructures, 1-15.
[29] Zeghoud, S., Hemmami, H., Seghir, B. B., Amor, I. B., Kouadri, I., Rebiai, A., ... & Simal-Gandara, J. (2022). A review on biogenic green synthesis of ZnO nanoparticles by plant biomass and their applications. Materials Today Communications, 104747.
[30] Lee, C. R., Kim, H. S., Jang, I. H., Im, J. H., & Park, N. G. (2011). Pseudo first-order adsorption kinetics of N719 dye on TiO2 surface. ACS applied materials & interfaces, 3(6), 1953-1957.
[31] Langmuir, I. (1918). The adsorption of gases on plane surfaces of glass, mica and platinum. Journal of the American Chemical society, 40(9), 1361-1403.
[32] Freundlich, H. M. F. (1906). Over the adsorption in solution. J. Phys. chem, 57(385471), 1100-1107.
[33] Al-darwesh, M. Y., Ibrahim, S. S., Naief, M. F., Mohammed, A. M., & Chebbi, H. (2023). Synthesis and characterizations of zinc oxide nanoparticles and its ability to detect O2 and NH3 gases. Results in Chemistry, 6, 101064.
[34] Sharma, A., Singh, B. P., Dhar, S., Gondorf, A., & Spasova, M. (2012). Effect of surface groups on the luminescence property of ZnO nanoparticles synthesized by sol–gel route. Surface Science, 606(3-4), L13-L17.
[35] Chamoli, P., Shukla, R. K., Bezbaruah, A. N., Kar, K. K., & Raina, K. K. (2021). Rapid microwave growth of mesoporous TiO2 nano-tripods for efficient photocatalysis and adsorption. Journal of Applied Physics, 130(16).
[36] Joseph, H. M., & Poornima, N. (2019). Synthesis and characterization of ZnO nanoparticles. Materials Today: Proceedings, 9, 7-12.
[37] Li, F., Ding, Y., Gao, P., Xin, X., & Wang, Z. L. (2004). Single‐crystal hexagonal disks and rings of ZnO: Low‐temperature, large‐scale synthesis and growth mechanism. Angewandte Chemie International Edition, 43(39), 5238-5242.
[38] Chamoli, P., Shukla, R. K., Bezbaruah, A. N., Kar, K. K., & Raina, K. K. (2021). Microwave-assisted rapid synthesis of honeycomb core-ZnO tetrapods nanocomposites for excellent photocatalytic activity against different organic dyes. Applied Surface Science, 555, 149663.
[39] Aljaafari, A., Ahmed, F., Awada, C., & Shaalan, N. M. (2020). Flower-like ZnO nanorods synthesized by microwave-assisted one-pot method for detecting reducing gases: structural properties and sensing reversibility. Frontiers in Chemistry, 8, 456.
[40] Zheng, Y., Fu, L., Han, F., Wang, A., Cai, W., Yu, J., ... & Peng, F. (2015). Green biosynthesis and characterization of zinc oxide nanoparticles using Corymbia citriodora leaf extract and their photocatalytic activity. Green Chemistry Letters and Reviews, 8(2), 59-63.
[41] Yousefi, R., Jamali-Sheini, F., Cheraghizade, M., Khosravi-Gandomani, S., Saaedi, A., Huang, N. M., ... & Azarang, M. (2015). Enhanced visible-light photocatalytic activity of strontium-doped zinc oxide nanoparticles. Materials Science in Semiconductor Processing, 32, 152-159.
[42] Nava, O. J., Soto-Robles, C. A., Gómez-Gutiérrez, C. M., Vilchis-Nestor, A. R., Castro-Beltrán, A., Olivas, A., & Luque, P. A. (2017). Fruit peel extract mediated green synthesis of zinc oxide nanoparticles. Journal of Molecular Structure, 1147, 1-6.
[43] Fu, L., & Fu, Z. (2015). Plectranthus amboinicus leaf extract–assisted biosynthesis of ZnO nanoparticles and their photocatalytic activity. Ceramics International, 41(2), 2492-2496. 
[44] Azarang, M., Shuhaimi, A., Yousefi, R., & Jahromi, S. P. (2015). One-pot sol–gel synthesis of reduced graphene oxide uniformly decorated zinc oxide nanoparticles in starch environment for highly efficient photodegradation of Methylene Blue. RSC Advances, 5(28), 21888-21896.
[45] Qais, D. S., Islam, M. N., Othman, M. H. D., Mahmud, H. E., Quayum, M. E., Islam, M. A., ... & Habib, A. (2023). Nano-zinc oxide fibers: Synthesis, characterization, adsorption of acid blue 92 dye, isotherms, thermodynamics and kinetics. Emerging Contaminants, 9(2), 100224.
[46] Chen, X., Zhang, F., Wang, Q., Han, X., Li, X., Liu, J., ... & Qu, F. (2015). The synthesis of ZnO/SnO 2 porous nanofibers for dye adsorption and degradation. Dalton Transactions, 44(7), 3034-3042.
[47] Farrokhi, M., Hosseini, S. C., Yang, J. K., & Shirzad-Siboni, M. (2014). Application of ZnO–Fe 3 O 4 nanocomposite on the removal of azo dye from aqueous solutions: kinetics and equilibrium studies. Water, Air, & Soil Pollution, 225, 1-12.
[48] Al-Arjan, W. S. (2022). Zinc oxide nanoparticles and their application in adsorption of toxic dye from aqueous solution. Polymers, 14(15), 3086.
[49] Zafar, M. N., Dar, Q., Nawaz, F., Zafar, M. N., Iqbal, M., & Nazar, M. F. (2019). Effective adsorptive removal of azo dyes over spherical ZnO nanoparticles. Journal of Materials Research and Technology, 8(1), 713-725.
[50] Singh, N., Shah, K., & Pramanik, B. K. (2023). Synthesis and application of manganese-doped zinc oxide as a potential adsorbent for removal of Congo red dye from wastewater. Environmental Research, 116484.
[51] Monsef Khoshhesab, Z., Gonbadi, K., & Rezaei Behbehani, G. (2015). Removal of reactive black 8 dye from aqueous solutions using zinc oxide nanoparticles: investigation of adsorption parameters. Desalination and Water Treatment, 56(6), 1558-1565.
[52] Elfeky, A. S., Youssef, H. F., & Elzaref, A. S. (2020). Adsorption of dye from wastewater onto ZnO nanoparticles-loaded zeolite: kinetic, thermodynamic and isotherm studies. Zeitschrift für Physikalische Chemie, 234(2), 255-278.