Document Type : Original Research Paper
Graphical Abstract
Highlights
1. Introduction
Steel materials are a crucial foundation of worldwide economic development and infrastructure construction; yet, their associated corrosion issues significantly reduce their service life, resulting in substantial economic losses and resource depletion, while also posing considerable risks to human safety [1]. Attaining superior corrosion resistance with traditional coatings in a high-humidity environment is challenging [2]. Currently, numerous methods such as the formulation of alloyed steel, electroplating, cathodic protection utilizing an external power source, and protective coatings are extensively employed to safeguard against steel corrosion [3-6]. Among these, anti-corrosion coatings have emerged as a crucial method due to their straightforward manufacture, broad applicability, cost-effectiveness, and favorable constructability [7]. Solvent-based epoxy coatings are extensively utilized for corrosion prevention owing to their superior adhesion and barrier characteristics [8]. During the curing process, microcracks and pores may occur, diminishing their long-term efficacy in adverse settings [9].
Among many inorganic nanomaterials, Zinc Oxide (ZnO) nanoparticles demonstrate distinct features such as high stability, low cost, and environmental friendliness [10], rendering them appealing candidates for multifunctional surface protection. ZnO serves as an efficient barrier filler in organic coatings, enhancing corrosion resistance by obstructing the ingress of water, oxygen, and chloride ions via a convoluted diffusion pathway. Furthermore, ZnO possesses the capability to mitigate corrosion via passivation and cathodic protection mechanisms. The efficacy of ZnO in corrosion prevention is affected by variables like particle shape, dispersion, and surface area [11]. Besides its recognized chemical and thermal durability, ZnO nanoparticles exhibit broad-spectrum antibacterial capabilities, principally due to the production of reactive oxygen species (ROS), a generally acknowledged mechanism for bacterial inactivation. Additional documented mechanisms encompass Zn²⁺ ion release, membrane rupture, and nanoparticle internalization. The antibacterial efficacy of ZnO is significantly influenced by particle size and dispersion. Smaller nanoparticles generally offer more surface area and improved antibacterial properties [12-14]. Moreover, the surface modification of ZnO nanoparticles with stearic acid can markedly augment their hydrophobicity, resulting in enhanced dispersion within the epoxy matrix and greater water-repellent, anticorrosive, and antibacterial properties [15].
Besides their anticorrosive capabilities, ZnO nanoparticles demonstrate extensive antibacterial activity. This is mainly due to the production of reactive oxygen species (ROS), which damage cellular components and result in bacterial death [16]. Alternative hypothesized pathways encompass Zn²⁺ ion release, membrane impairment, and nanoparticle uptake. The antibacterial efficacy of ZnO is significantly influenced by particle size and dispersion. Minuscule and uniformly distributed nanoparticles provide increased surface interaction with microbial cells, hence augmenting the antibacterial efficacy [11–13].
Recent research has shown that zinc oxide (ZnO) nanoparticles can be used to make coatings that do more than one thing, including protect against corrosion and have antibacterial properties. Feng et al. [17] made zinc coatings that are superhydrophobic and antifouling by changing their surface using stearic acid. This shows how important hierarchical surface topography and lower surface energy are. Zhu et al. [15] showed that adding ZnO nanorods to composite matrices can greatly lower the rate of corrosion and make barriers work better, but this depends on how the nanorods are spread out and lined up. Qing et al. [18] showed that ZnO nanoflowers were better at preventing corrosion because they had a larger surface area and more complicated diffusion paths. He et al. [19] recently made ZnO–Al₂O₃ nanocomposite coatings by anodic oxidation and putting ZnO nanoparticles on top of each other. After 40 days of exposure, heat treatment at 250 °C led to a significant decrease in corrosion current density (1.127×10⁻⁸ A/cm²) and over 97% antibacterial effectiveness. This was due to a porous structure that made it easier for Zn²⁺ to escape and increased interfacial bonding. In addition, Jlassi et al. [20] made hybrid nanocomposites with ZnO, polypyrrole, and clay that had both anticorrosion and antibacterial capabilities. These properties came from combining organic and inorganic phases and strengthening conductive polymers. All of these studies agree that changing the shape and adding functional groups to the surface are important ways to make ZnO-based nanomaterials better for dual-function coatings. There aren’t many complete studies that use both methods on different types of ZnO, especially when they look at both electrochemical and microbiological factors at the same time. This shows that there is a big need for more research in this area, which this study attempts to fill.
The present study explores the dual functionality of zinc oxide (ZnO) nanomaterials in corrosion protection and antimicrobial activity, focusing on the influence of particle morphology and surface chemistry. Two morphologies of ZnO (spherical and rod-shaped) were synthesized and subsequently modified with stearic acid (SA) to enhance hydrophobicity and dispersion stability. Although ZnO nanostructures have been widely investigated for either corrosion resistance or antibacterial properties, limited research has addressed the combined effects of morphological engineering and surface modification on both functionalities. In this work, the nanomaterials were integrated into protective systems and characterized using structural, electrochemical, and microbiological techniques to evaluate performance. The findings reveal a functional trade-off between corrosion inhibition and antibacterial efficacy, offering insights for the rational design of multifunctional ZnO-based coatings applicable in industrial and biomedical contexts.
2. Experimental
2.1. Materials and chemicals
Zinc acetate dihydrate (Zn(CH₃COO)₂·2H₂O), sodium hydroxide (NaOH), and stearic acid (C₁₈H₃₆O₂) were purchased from Merck and were used without further purification. Absolute ethanol (C₂H₅OH) was used as a solvent in both synthesis and surface modification processes. All reagents were of analytical grade. Deionized (DI) water was used throughout all experimental procedures. Mild steel plates (grade SC37, equivalent to ASTM A36 / DIN St37-2), with iron content above 98.5%, were used as metallic substrates for corrosion testing. Agar powder, nutrient broth, and bacterial strains of Escherichia coli (E. coli) and Staphylococcus aureus (S. aureus) were obtained from the Iranian Biological Resource Center (IBRC) for antibacterial assays.
2.2. Material preparation
2.2.1. Synthesis of ZnO Nanoparticles
Rod-like ZnO nanoparticles were made using a method called homogeneous precipitation. Separate solutions were made of zinc nitrate hexahydrate (0.1 M) and hexamethylenetetramine (HMT, 0.1 M), and then mixed while agitating them with a magnet at 80 °C for 12 hours. The white precipitate that formed was recovered by centrifugation, washed with deionized water and ethanol multiple times, and then dried in a vacuum oven at 80 °C for 12 hours. This unmodified rod-like ZnO sample was called ZnO-R.
Spherical ZnO nanoparticles were synthesized using a hydrothermal technique. A homogenous suspension was made by stirring together 2.74 g of zinc acetate dihydrate, 2.4 g of citric acid, and 60 mL of 1 M NaOH for 30 minutes. We put the mixture in a 100 mL Teflon-lined autoclave and cooked it at 160 °C for 4 hours. After letting the precipitates drop down to ambient temperature, they were centrifuged and thoroughly cleaned. Then, they were dried in a vacuum at 60 °C until they reached a consistent weight. The unaltered spherical ZnO sample was called ZnO-S.
2.3. Surface Modification of ZnO Nanoparticles
To augment hydrophobicity and boost dispersion stability, both rod-shaped and spherical ZnO nanoparticles were surface-functionalized with stearic acid. In summary, 0.2 g of ZnO nanoparticles were suspended in 60 mL of ethanol with stearic acid under ultrasonic agitation for 30 minutes. The mixture was subsequently magnetically agitated at 70 °C for 12 hours to promote the interaction between the hydroxyl groups on the ZnO surface and the carboxyl groups of stearic acid. The hydrophobically modified nanoparticles were subjected to multiple washes with ethanol to eliminate unbound stearic acid and subsequently dried under vacuum at 120 °C until a consistent weight was achieved. The functionalization method created a monolayer of stearic acid on the ZnO surface, converting the initially hydrophilic surface into a superhydrophobic contact. The altered rod-shaped and spherical specimens were designated as SA@ZnO-R and SA@ZnO-S, respectively.
2.4. Preparation of Coated Steel Samples
The mild steel plates (SC37, 2 × 2 cm²) were polished with grit 400–1200, washed with ethanol and deionized water, and then dried. Epoxy and hardener were combined in a 2:1 weight ratio, and then added 2% by weight of either unmodified or stearic acid-modified ZnO was added. Then, the mixture was ultrasonicated for 15 minutes. The coatings were put on by drop-casting and then dried for two hours at 60 °C. Four samples were analyzed: (1) bare steel, (2) epoxy-coated steel, (3) SA@ZnO-R/epoxy, and (4) SA@ZnO-S/epoxy, to assess the impact of ZnO morphology and surface modification on protection performance.
2.5. Characterization Techniques
The morphology and particle size of ZnO nanoparticles were observed using field-emission scanning electron microscopy (FE-SEM, MIRA3 TESCAN, Czech Republic). The crystalline structure was determined by X-ray diffraction (XRD, X’Pert PRO MPD, Netherlands) with Cu Kα radiation (λ = 1.5406 Å). Surface functional groups and chemical bonding were analyzed using Fourier-transform infrared spectroscopy (FTIR, NICOLET iS10, USA) in the range of 400–4000 cm⁻¹ [21-24].
Electrochemical corrosion performance of the coated and uncoated samples was evaluated in 3.5 wt.% NaCl solution at room temperature using a potentiostat/galvanostat (AUTOLAB, Netherlands) with a standard three-electrode cell configuration: the coated steel sample as the working electrode (exposed area: 1 cm²), a platinum wire as the counter electrode, and a saturated calomel electrode (SCE) as the reference electrode. Open-circuit potential (OCP) was recorded over a period of 30 minutes to assess the system’s stability and corrosion tendency. Tafel polarization measurements were then conducted in the potential range of ±250 mV vs. OCP at a scan rate of 1 mV/s. The corrosion potential (Ecorr) and corrosion current density (Icorr) were determined by extrapolating the linear portions of the anodic and cathodic branches of the polarization curve using Tafel fitting. The Icorr values were used to calculate the corrosion rate (CR) in mm/year according to Equation 1:
CR= (1)
where EW is the equivalent weight (g/equiv), ρ is the density (g/cm³), and A is the area of the exposed surface (cm²).
Electrochemical impedance spectroscopy (EIS) was performed at OCP over a frequency range of 100 kHz to 0.01 Hz with a 10 mV AC perturbation. The impedance data were analyzed using equivalent circuit modeling to find key parameters such as charge transfer resistance (Rct) and coating resistance (Rc). Higher Rct values indicate enhanced corrosion resistance due to improved barrier properties. The double-layer capacitance (Cdl) was calculated from the constant phase element (CPE) parameters using Equation 2:
Cdl=(Y0Rctn−1(2)
Where Y0 and n are obtained from the fitted Constant Phase Element (CPE), and Rct represents the charge transfer resistance. A reduction in Cdl indicates a diminished active surface area and enhanced protective properties of the coating.
The electrochemical investigations yielded detailed insights into the protective mechanisms and performance variations among the produced samples.
2.6. Antibacterial Activity Test
The antibacterial efficacy of the coated samples was assessed by the disk diffusion method against Escherichia coli (Gram-negative) and Staphylococcus aureus (Gram-positive) bacterial strains. New cultures of each bacterium were established by inoculating the nutritional broth and incubating it at 37 °C for 24 hours. A sterile cotton swab was employed to uniformly distribute the bacterial suspension across the nutrient agar plates. Circular coated specimens (2 × 2 cm²) were meticulously positioned on the agar surface and incubated at 37 °C for an additional 24 hours. The diameter of the inhibitory zone surrounding each sample was measured with a digital caliper. The presence and dimensions of the clear zone signified the sample’s efficacy in inhibiting bacterial proliferation [25, 26].
3. Results and Discussions
3.1. Characterization of ZnO nanoparticle
The FTIR spectra of ZnO-R and ZnO-S (Fig. 1-a) show prominent Zn–O stretching bands below 600 cm⁻¹, confirming the formation of ZnO crystalline structures. Broad absorption bands around 3400 cm⁻¹ in both samples indicate surface hydroxyl groups or adsorbed moisture, while signals near 1609 and 1376 cm⁻¹ are linked to H–O–H bending and C–O vibrations. Notably, these bands were a little stronger in ZnO-S, which may have been because it has a larger surface area and polarity, which makes it better at absorbing moisture [27, 28]. After modifying stearic acid (Fig.1-b), both SA@ZnO-R and SA@ZnO-S showed clear peaks at 2911 and 2848 cm⁻¹, which were due to the stretching of C–H bonds in alkyl chains. These features, absent in unmodified samples, confirm successful organic functionalization. The asymmetric and symmetric carboxylate bands at 1531 and 1458 cm⁻¹, with a ~73 cm⁻¹ difference, suggest bidentate coordination between the acid and surface Zn²⁺ ions. Compared to the unmodified samples, the significant spectral changes, especially in the 1000–3000 cm⁻¹ range, demonstrate successful chemical bonding without altering the ZnO core, as the Zn–O peak intensity remained largely unaffected [29].
The XRD patterns of ZnO-R, ZnO-S, SA@ZnO-R, and SA@ZnO-S are shown in Fig. 2. All of the samples had diffraction peaks at 2θ ≈ 31.7°, 34.5°, 36.2°, 47.5°, 56.6°, 62.8°, and 67.8°, which are the (100), (002), (101), (102), (110), (103), and (112) planes of the hexagonal wurtzite ZnO structure (JCPDS card no. 36-1451), confirming successful synthesis without secondary phases [30]. The ZnO-R sample showed a pronounced (002) peak, indicating preferred growth along the c-axis, which is consistent with its rod-like morphology. In contrast, the peak intensities of ZnO-S were more evenly distributed, reflecting isotropic crystal growth in line with its spherical shape. After surface modification, SA@ZnO-R and SA@ZnO-S retained all characteristic peaks of ZnO, showing that the core crystalline structure remained intact. However, a noticeable reduction in peak intensity, particularly in SA@ZnO-S, was shown. This can be attributed to the formation of an amorphous organic layer on the nanoparticle surfaces, which dampens X-ray reflection. The more significant decrease in SA@ZnO-S suggests better surface coverage due to its higher surface contact area, supporting the effectiveness of surface functionalization [31].
Fig. 3 presents SEM micrographs of ZnO-R, ZnO-S, SA@ZnO-R, and SA@ZnO-S nanoparticles. The ZnO-R sample displays elongated rod-like structures with uniform diameters and considerable aspect ratios, suggesting anisotropic development along the c-axis. This directional morphology corresponds with the prominent (002) diffraction peak identified in the XRD data, indicating a preferred crystal orientation.
Conversely, ZnO-S exhibits almost spherical nanoparticles characterized by a restricted size distribution and a smooth, compact surface. The isotropic crystal formation shown by the uniform intensity of XRD peaks aligns with this shape. The particles seem more aggregated while displaying a uniform size distribution, indicating regulated nucleation and growth conditions.
The original morphologies of the surface-modified samples were predominantly preserved. Both SA@ZnO-R and SA@ZnO-S exhibit alterations in surface texture. Specifically, SA@ZnO-S displays a more coated and indistinct surface, indicating the existence of a stearic acid layer. Likewise, SA@ZnO-R exhibits a somewhat rougher surface than its unmodified equivalent. The morphological changes validate the efficacy of surface modification, offering visual proof of organic layer creation while preserving the core structure of the nanoparticles.
3.2. Electrochemical Corrosion Evaluation
Fig. 4 shows the OCP curves (In a 3.5 wt.% NaCl solution) of both the coated and uncoated samples. The SA@ZnO-S sample had the highest and most steady potential (around +0.10 V), which means it was the most resistant to corrosion and passive. The better performance is due to the even distribution of spherical ZnO nanoparticles treated with stearic acid. These nanoparticles form a tight, water-repelling barrier that keeps chloride ions from getting through. SA@ZnO-R had a greater negative potential (around −0.35 V), which means it was somewhat resistant to corrosion. Compared to spherical particles, the rod-like shape may make the particles less evenly spread out and make the barrier less strong. Still, this sample did better than both the epoxy-only and bare metal samples because ZnO has an inherent inhibitive effect. The OCP of the epoxy-coated steel was more negative and unstable (≈ −0.55 V), which means that the coating was more permeable and had more local flaws. The naked sample had the lowest and most variable potential (−0.60 V), which showed that it was very likely to corrode in the salty environment. Overall, these results show that SA@ZnO-S offers better protection because of both effective surface modification and the way the nanoparticles are shaped.
Fig. 5 shows the Tafel polarization curves for the coated and untreated samples in a 3.5 wt.% NaCl solution. Table 1 lists the most important electrochemical parameters. These measurements provide insights into corrosion potential (Ecorr), corrosion current density (icorr), polarization resistance (Rp), and inhibition efficiency (η). Among all samples, SA@ZnO-S had the highest Ecorr (+0.10 V) and the lowest icorr (1.18 µA/cm²), indicating exceptional corrosion resistance. The corrosion rate of 0.013 mm/year and elevated polarization resistance of 12,237.87 Ω·cm² signify the formation of a dense and passive barrier due to the uniform distribution of spherical ZnO nanoparticles treated with stearic acid. The inhibitory efficiency attained 75.82%, validating the synergistic impact of nanoparticle shape and surface modification. The SA@ZnO-R sample exhibited modest performance, with Ecorr at −0.35 V and icorr at 1.86 µA/cm². Notwithstanding its reduced efficiency (61.89%) relative to SA@ZnO-S, it nonetheless surpassed the epoxy and control samples. The rod-like architecture may have led to less uniform dispersion and diminished surface coverage, hence decreasing barrier efficacy. The epoxy-only coating exhibited inadequate protection, characterized by a greater icorr (2.56 µA/cm²), a lower Rp (5,652.44 Ω·cm²), and an efficiency of 47.54%. This indicates inadequate resistance to electrolyte infiltration and micro-defect development. The Control sample exhibited the most inferior performance, with an icorr of 4.88 µA/cm² and the lowest Rp of 2,589.49 Ω·cm², thereby affirming its susceptibility to corrosion. These findings highlight the essential significance of nanoparticle shape and surface chemistry. The SA@ZnO-S coating, characterized by its hydrophobic, compact, and well-dispersed nanostructure, demonstrated superior corrosion resistance, evidenced by a markedly decreased icorr, elevated Rp, and favorable Ecorr.
Fig. 6 and Table 2 present the Nyquist plots of the tested samples in 3.5 wt.% NaCl solution. The semicircle diameter correlates with corrosion resistance, where a larger diameter indicates higher charge-transfer resistance (Rct) and improved barrier properties. Of all coatings, SA@ZnO-S exhibited the largest semicircle, signifying the highest Rct (26,125 Ω·cm²) and outstanding corrosion resistance. The enhanced performance results from the uniform, dense coating formed by spherical ZnO nanoparticles and stearic acid, which effectively restricts charge transfer at the metal–electrolyte interface. Additionally, the coating resistance (Rc) for this sample reached 12,580 Ω·cm², confirming strong barrier integrity. SA@ZnO-R showed a moderate improvement, with Rct and Rc values of 5,567 Ω·cm² and 3,224 Ω·cm², respectively. The relatively lower protection may be due to the rod-like morphology, which limits nanoparticle packing density and dispersion uniformity, resulting in localized defects. The epoxy-only coating demonstrated a smaller semicircle, with Rct of 3,372 Ω·cm² and Rc of 1,825 Ω·cm². This suggests moderate barrier performance, likely compromised by microvoids and electrolyte permeation. The uncoated steel sample (Control) demonstrated the lowest diameter (Rct = 1,382 Ω·cm²), underscoring its significant vulnerability to corrosion in the saltwater environment. The constant phase element of the double layer (CPEdl) for SA@ZnO-S was markedly diminished (1.02 × 10⁻⁹ Ω⁻¹·cm²·sⁿ), signifying less interaction between the electrolyte and the metal surface. This facilitates the development of a compact, hydrophobic layer that hinders electrolyte infiltration and charge transfer. The amalgamation of an elevated ZnO dielectric constant and hydrophobic stearate chains synergistically improves the overall protective efficacy.
3.3. Antibacterial Activity Evaluation
The antibacterial efficacy of ZnO-based nanoparticles was assessed by the agar disk diffusion method against Staphylococcus aureus (Gram-positive) and Escherichia coli (Gram-negative). Samples comprising ZnO-R, ZnO-S, SA@ZnO-R, and SA@ZnO-S were evaluated in powdered form. Following a 24-hour incubation at 37 °C, the sizes of the inhibitory zones were determined (Fig. 7, Table 3). Pristine ZnO-S exhibited the highest antibacterial efficacy, with inhibition zones of 4.7 cm (S. aureus) and 4.19 cm (E. coli), followed by ZnO-R. The enhanced performance of ZnO-S is likely due to its higher surface area and isotropic morphology, promoting efficient Zn²⁺ ion release and ROS generation. In contrast, stearic acid–modified samples (SA@ZnO-R and SA@ZnO-S) demonstrated reduced antibacterial activity. The organic coating likely limited ion release and surface interactions, acting as a diffusion barrier to ROS. Notably, SA@ZnO-S still outperformed SA@ZnO-R, possibly due to its better particle dispersion and surface coverage. All samples showed greater inhibition against S. aureus, consistent with the higher susceptibility of Gram-positive bacteria to ZnO, attributed to their thicker peptidoglycan layers and lack of outer membrane. These results highlight a trade-off: while surface modification improves corrosion resistance, it partially compromises antibacterial performance by hindering the active release of antimicrobial agents.
Zinc oxide nanoparticles (ZnO NPs) exert their antibacterial activity through multiple, interrelated mechanisms. One major pathway involves the generation of reactive oxygen species (ROS) such as hydrogen peroxide (H₂O₂), hydroxyl radicals (•OH), and superoxide anions (O₂⁻), which induce oxidative stress and cause damage to proteins, lipids, and DNA inside bacterial cells. In addition, ZnO can release Zn²⁺ ions into the surrounding medium, which interfere with bacterial enzyme systems and metabolic functions. Another important mechanism is the direct interaction of ZnO NPs with the bacterial cell membrane, leading to increased membrane permeability, structural disruption, and eventual cell lysis. These combined effects make ZnO nanostructures effective against both Gram-positive and Gram-negative bacteria, although the extent of activity may vary depending on the morphology, surface chemistry, and concentration of the nanoparticles [32, 33].
Table 4 compares the corrosion inhibition efficiency and antibacterial performance of the synthesized ZnO-based nanomaterials in this study with selected peer-reviewed reports. Surface modification with stearic acid improves corrosion protection (ηinh ≈ 93.2%), while unmodified ZnO shows stronger antibacterial efficacy. These values are in agreement with prior studies utilizing green or bimetallic ZnO structures, highlighting the importance of morphology and surface chemistry optimization.
4. Conclusion
This study conducted a comparative analysis of the corrosion resistance and antibacterial performance of ZnO nanoparticles with two distinct morphologies (rod-like (ZnO-R) and spherical (ZnO-S)), both in their pristine and stearic acid-modified states. The results clearly demonstrated that the morphology and surface chemistry of ZnO nanostructures play a critical role in determining their dual functionality. Among all tested configurations, the stearic acid-modified spherical ZnO (SA@ZnO-S) exhibited the optimum performance in terms of corrosion resistance, as confirmed by electrochemical measurements including OCP, Tafel, and EIS. This superior behavior was attributed to its uniform dispersion, compact surface coverage, and enhanced hydrophobicity, leading to reduced corrosion current density and increased charge transfer resistance. Conversely, unmodified ZnO-S and ZnO-R showed superior antibacterial activity, likely due to enhanced Zn²⁺ ion release and ROS generation, which are partially restricted in surface-modified samples due to the diffusion-limiting effect of the hydrophobic layer. These findings reveal a critical trade-off between corrosion protection and antibacterial efficacy, governed by both morphology and surface modification. The significance of this work lies in its systematic exploration of how nanoscale morphological engineering and organic surface functionalization influence multifunctional coating behavior. Unlike many previous studies focusing on either corrosion resistance or antibacterial activity, this research presents an integrated strategy to tailor both properties simultaneously. This dual-functionality framework offers valuable guidance for the design of ZnO-based nanocoatings with targeted performance in biomedical, marine, and industrial environments, where both bioactivity and material durability are essential.
Acknowledgements
The authors express their gratitude to the Babol Noshirvani University of Technology for their generous provision of financial support (BNUT) for the completion of this survey.
Conflict of Interest
The authors declare no conflict of interest.
Funding
This study was not supported by any funding.
Author’s Contributions
Study Conception or Design: HMS; MG
Data Acquisition: HMS
Data Analysis or Interpretation: HMS; MG
Manuscript Drafting: HMS
Critical Manuscript Revision: MG
All authors have approved the final manuscript and are responsible for all aspects of the work.
AI Statement