Document Type : Original Research Paper
Graphical Abstract
INTRODUCTION
Environmental safety is a critical global concern, particularly in relation to water pollution [1]. The contamination of water bodies by pollutants such as heavy metals, synthetic dyes, and pesticides presents serious risks to both aquatic ecosystems and human health [2]. Among these pollutants, organic dyes originating from industrial processes such as textile manufacturing, food processing, cosmetics, and pharmaceuticals are of particular concern due to their high stability, toxicity, and resistance to biodegradation [3]. Methylene blue (MB), a commonly used cationic dye, has been classified as a priority pollutant because of its mutagenic and carcinogenic properties [4]. Several conventional methods, including ion exchange, chemical oxidation, ozonolysis, and advanced oxidation processes (AOPs), have been explored for dye removal. However, among these, photocatalytic degradation using semiconductor nanomaterials stands out due to its cost-effectiveness, reusability, and environmental sustainability [5]. Metal oxide photocatalysts such as nickel oxide, copper oxide (CuO), and titanium dioxide (TiO₂) are widely investigated for their ability to generate reactive oxygen species (ROS) under UV or visible light irradiation [6], [7]. CuO-TiO₂ nanocomposites, in particular, have attracted attention for their enhanced photocatalytic efficiency, affordability, low toxicity, and high photostability [8]. The narrow bandgap of CuO (~1.2 eV) enables visible light absorption, while the wide bandgap of TiO₂ (~3.0–3.2 eV) contributes to structural stability and electron transport [9]. Their synergistic interaction facilitates effective charge separation and reduces electron–hole recombination, improving photocatalytic performance. Despite these advancements, most synthesis methods for CuO-TiO₂ nanocomposites rely on energy-intensive processes involving hazardous chemicals, which raise environmental and health concerns [10]. Recently, green synthesis methods have gained prominence as a sustainable alternative, using plant extracts rich in phytochemicals to mediate the formation of nanomaterials in a non-toxic, low-cost, and eco-friendly manner [11][12]. While various plant species have been employed in nanoparticle synthesis, the application of Hibiscus sabdariffa (HS) flower extract as a reducing and stabilizing agent for synthesizing CuO-TiO₂ nanocomposites remains underexplored. The novelty of this work lies in the use of HS flower extract for the first-time green synthesis of CuO–TiO₂ nanocomposites, specifically applied for MB degradation under UV irradiation. Unlike previous studies, this research incorporates detailed physicochemical characterization and evaluates not only photocatalytic performance but also potential ecological impact through brine shrimp (Artemia sp.) toxicity assays. This integrated approach addresses the growing need for eco-friendly materials in environmental remediation while contributing novel insights into the safe application of nanocomposites in aquatic environments.
In addition, this study investigates photocatalytic activity under controlled parameters (pH, temperature, time) to optimize degradation efficiency, providing a model for reproducibility and future scale-up. This study presents, for the first time, green-synthesized CuO-TiO₂ nanocomposites utilizing HS extract, exhibiting effective degradation of MB dye. This method provides environmental safety, economic efficiency, and biocompatibility. The CuO–TiO₂ nanocomposites also offer an accessible alternative for developing countries where industrial dye pollution is prevalent, yet resources for advanced treatment technologies are limited. In summary, this research addresses a critical gap in sustainable nanotechnology by offering a green, non-toxic, and cost-effective synthesis route for high-performance photocatalysts, along with an assessment of their environmental safety, an aspect often overlooked in similar studies.
All chemicals utilized were of analytical grade and employed without additional purification
The organic materials and chemicals with relevant information in this research were as follows:
For the preparation of plant extracts, HS flowers were procured from local markets in Zuru Local Government Area, Kebbi State, Nigeria. Copper(II) chloride dihydrate (CuCl₂·2H₂O) with a purity of ≥ 99% was procured from SYSTEM, Malaysia. Titanium(VI) oxide (TiO₂) with a purity of ≥99% was obtained from R&M Chemicals, Malaysia. Sodium hydroxide (NaOH) with 98% purity was obtained from R&M Chemicals, London, UK, polyethylene glycol (PEG) HO(C2H4O)nH, 1,800 g/mol with a purity of ≥ 99% was purchased from Merck KGaA,64271 Darmstadt Germany and acetone (C₃H₆O) with a quality grade of QP (purity ≥ 99.5%) was purchased from HmbG Chemicals, Malaysia. In the photocatalytic activity experiments, MB (C₁₆H₁₈ClN₃S) with a molar mass of 319.86 g/mol and a purity of ≥ 98%, was acquired from Merck, Malaysia. Brine shrimp (A. salina) cysts were provided by the Integrated Chemical Biophysics Research Unit, Faculty of Science, Universiti Putra Malaysia. Distilled water was used for all experimental procedures.
Initially, fresh HS flowers were obtained from Zuru local government area, Kebbi state, Nigeria, and carefully washed with tap water to remove any surface impurities. The cleaned flowers were air-dried at room temperature in a shaded environment to prevent degradation. After drying, the flowers were ground into a fine powder using a grinder, and the resulting powder was set aside for subsequent use. To prepare the leaf extract intended to act as a reducing, capping, or stabilizing agent, 10 g of the powdered flowers were combined with 100 mL of distilled water. This mixture was heated to 80°C and continuously stirred on a hotplate with a magnetic stirrer for 40 minutes. Following heating, the solution was filtered using Whatman No. 1 filter paper, and the extract was stored at 4°C for future application in nanocomposites synthesis as a reducing agent.
Synthesis of biogenic CuO-TiO2 nanocomposite
The synthesis of the CuO-TiO₂ nanocomposite employs a modified green synthesis approach, based on the methodology described by [13]. Initially, 1.36 g of CuCl₂·2H₂O is dissolved in 80 mL of distilled water and stirred for 10 minutes. Subsequently, 25 mL of HS flower extract is added dropwise to the solution. NaOH is gradually introduced to adjust the pH to 12 while maintaining continuous stirring at 250 rpm. The reaction mixture is stirred for 8 hours to ensure thorough interaction. After completion of the stirring process, the suspension is centrifuged at 6000 rpm for 15 minutes, and the resulting precipitate is washed three times with acetone to achieve high purity. The synthesized CuONPs are then dried in an oven at 60 °C for 48 hours and ground into a fine powder, as depicted in Figure 1.
The synthesis of TiO₂NPs follows a similar process. Here, 1.6 g of TiO₂ is dispersed in 80 mL of distilled water and stirred for 10 minutes. Then, 25 mL of HS powder extract is gradually added to the solution. NaOH is introduced dropwise to adjust the pH to 11, with stirring maintained at 250 rpm. The mixture is stirred for 4 hours at 30°C to facilitate the reaction. The resulting suspension is centrifuged at 6000 rpm for 15 minutes, and the precipitate is washed three times with acetone to ensure a high degree of purity. The TiO₂NPs are subsequently dried in an oven at 60°C for 48 hours and ground into a fine powder. Figure 1 illustrates the synthesis procedure. Notably, no calcination step is employed, preserving the organic compounds from the plant extract that function as reducing and capping agents during synthesis. This approach successfully yields pure CuONPs and TiO₂NPs, which are then combined in a 1:1 mass ratio to fabricate the CuO-TiO₂ nanocomposites.
Characterization of CuO-TiO₂ nanocomposite
The CuO-TiO₂ nanocomposites were analyzed using various techniques to thoroughly understand their crystal structure, morphology, oxidation states, and thermal stability [14]. The triple-axis diffractometer synchrotron X-ray diffraction (XRD) (Jordan Valley Bede D1 X-ray diffractometer) was employed to determine the crystal structure of the CuO-TiO₂ nanocomposites, while their morphology was examined using field emission scanning electron microscopy (FESEM) on a FEI Nova NanoSEM 450. Energy dispersive X-ray spectroscopy (EDS) with a Bruker XFlash 6I30 detector was used to analyze the elemental composition and oxidation states of the nanocomposites by measuring the emitted X-rays [15]. Functional groups in the CuO-TiO₂ nanocomposites were identified through Fourier-transform infrared spectroscopy (FTIR) using a Perkin Elmer FTIR-spectrum 400. The average particle size and size distribution in suspension were measured using dynamic light scattering (DLS) with a Malvern Zetasizer (USA). Photoluminescence (PL) measurements, taken using an Edinburgh Instrument, provided data on the photo-generated energy of the CuO-TiO₂ nanocomposites. The surface area and porosity were assessed through the Brunauer–Emmett–Teller (BET) theory, which analyzes the physical adsorption of gas molecules on the nanocomposite surface. Thermogravimetric analysis (TGA) was conducted using a Mettler Toledo TGA/SDTA 851 to determine decomposition and mass loss over a range of temperatures. Differential thermal analysis (DTA) was also performed to identify endothermic and exothermic events, as well as phase transitions [16], and Gas Chromatography Mass Spectrometry (GC-MS) (GC-MS-QP2010 Plus). Finally, the photocatalytic degradation performance of the CuO-TiO₂ nanocomposite was evaluated using UV-light spectrophotometry to monitor the degradation process [17].
The CuO-TiO₂ nanocomposites were prepared using a one-pot reaction method. Initially, 1 g of PEG was dissolved in 50 mL of distilled water under continuous stirring at 400 rpm for 30 minutes to ensure complete dissolution. PEG acted as a dispersing medium to promote uniform mixing of the NPs. Subsequently, 3 g of as-synthesized CuONPs were added to the PEG solution and stirred for 1 hour to achieve a well-dispersed suspension. Following this, 3 g of TiO₂NPs were equally introduced into the mixture [18]. The system was maintained at 70°C and stirred at 400 rpm for an additional 1 hour to ensure homogeneity and facilitate the composition process, leading to the formation of the CuO-TiO₂ nanocomposites. The resultant composites were washed three times with acetone to remove impurities and any unreacted materials. The solid product was separated by centrifugation at 6000 rpm for 15 minutes and subsequently oven-dried at 60°C for 48 hours to obtain the final CuO-TiO₂ composites. Figure 2 illustrates the synthesis process of CuO-TiO2 nanocomposites. This synthesis approach allows for the effective composition of CuONPs into the TiO₂NPs matrix, enhancing the photocatalytic activity of the composite material by combining the unique properties of both components [19].
Study of Photocatalytic Degradation
A total of 20 mg of MB was dissolved in 1 liter of distilled water. Then, 100 mL of dissolved dye was taken to a 250mL beaker. 10 mg of CuO-TiO2 nanocomposite powder was dissolved in 100 mL of dye solution and continuously stirred for 30 min till adsorption adsorption-desorption equilibrium was achieved. UV lamps that primarily emit a power of 30 W (about 400 luminous light intensity) and 220 V were applied as a source of visible light and situated parallel to the reactor [20]. Then, the absorbance of the solutions was recorded every 20 minutes using a UV–Vis spectrophotometer. The percentage degradation efficiency of the photocatalysts was calculated as follows [21]:
where C0 is the dye initial concentration, C is the concentration of dye at time “t,” A0 is the absorbance at the initial stage, and At is the absorbance of dye at time “t.” The wavelength of light corresponding to the maximum absorbance of MB is found to be 668 nm and measured accordingly. The degradation kinetics of MB dye were studied using the initial times of 20, 40, 60, 80, 100, 120, 140, and 160 min. The catalytic activity of as-synthesized photocatalysts under UV–light can be evaluated by comparing the apparent rate constants [22]. Accordingly, the degradation kinetics is also described using pseudo-first-order (Equation (2)).
where Co and C represent the initial and time-dependent concentrations of respectively, and K1 is the rate constant for the pseudo-first-order kinetic model [23]. Table 1 summarizes key physicochemical properties of MB, a commonly used cationic dye in photocatalytic degradation studies.
Brine Shrimp Lethality Assay (BSLA)
The cytotoxicity of CuO-TiO2 nanocomposites was evaluated in brine shrimp larvae using established methods [32]. A lethality assay was conducted by preparing a stock solution of CuO-TiO2 nanocomposites in distilled water and making fresh suspensions at varying concentrations (0.1–1 mg/mL) through serial dilution in artificial seawater. A volume of 200 μL of each concentration was added to wells of a 96-well plate, followed by the addition of 10 nauplii per well. The plates were incubated at room temperature (26–28°C) for 24 hours. After the incubation period, the number of surviving nauplii in each well was counted under a microscope. Negative control wells contained 10 nauplii and artificial seawater without CuO-TiO2 nanocomposites. Experiments were conducted in triplicate for each concentration. The percentage of mortality was determined by comparing the number of survivors in the test and control wells, and lethality was calculated using Abbott’s formula:
The synchrotron XRD pattern of the CuO-TiO₂ nanocomposites exhibits distinct diffraction peaks corresponding to both CuONPs and TiO₂NPs phases. The prominent peaks at 2θ values around 25.3°, 37.8°, and 48.0° can be attributed to the anatase phase of TiO₂NPs, indexed to (101), (004), and (200) planes, respectively, as per the standard JCPDS file (No. 21-1272) [33]. The characteristic peaks corresponding to CuONPs are observed at 2θ values around 35.5°, 38.7°, and 48.7°, which can be indexed to the (111), (200), and (202) planes, aligning with the JCPDS file (No. 48-1548) as illustrated in Figure 3 [34]. The presence of peaks from both TiO₂NPs and CuONPs phases confirms the successful formation of the CuO-TiO₂ nanocomposite. The absence of impurity peaks in the XRD pattern indicates the purity of the synthesized material. Furthermore, the sharp and well-defined peaks suggest a high degree of crystallinity, which is crucial for enhanced photocatalytic performance [35]. The diffraction peak broadening is indicative of the nanoscale dimensions of the synthesized composite. The size of 108 nm was determined using Scherrer’s formula [36].
The observed synergistic incorporation of CuONPs and TiO₂NPs enhances the composite’s potential for photocatalytic applications, particularly in wastewater remediation [37].
Fourier transform infrared spectroscopy analysis
The FT-IR spectrum provided for CuO-TiO₂ nanocomposite presents significant peaks that can be associated with various molecular vibrations within the material. Broad absorption at 3379 cm⁻¹, this region typically corresponds to the O-H stretching vibrations, which suggest the presence of hydroxyl groups (–OH) likely due to surface adsorbed water or hydroxyl groups on the CuO-TiO₂ nanocomposite surface. The broad nature of the peak indicates hydrogen bonding. Peaks at 1600 cm⁻¹, these can be attributed to the bending vibration of molecular water (H-O-H). These vibrations occur due to water molecules adsorbed onto the surface of the composite material. Peaks within 1089-1384 cm⁻¹, these regions are indicative of C-O stretching vibrations [38]. The presence of such vibrations might be due to residual carbon-containing impurities from the synthesis or preparation process. The region below 1000 cm⁻¹ typically shows absorption bands corresponding to metal–oxide vibrations. The peaks in this area, especially around 516-640 cm⁻¹, are characteristic of Ti-O-Ti and Cu-O bond stretching modes as shown in Figure 4. These vibrations confirm the presence of both TiO2NPs and CuONPs in the nanocomposite structure. Ti-O stretching generally appears around 516-640 cm⁻¹ and signifies the TiO₂NPs lattice vibrations. Cu-O stretching is expected around a similar region, confirming the integration of CuONPs into the material. The whole transmittance pattern suggests that the nanocomposite material of CuO-TiO₂ has been successfully formed, with key functional groups corresponding to both oxides clearly evident [39]. The presence of adsorbed water and possible surface hydroxyl groups also indicates interaction with the environment, which could affect surface properties such as photocatalytic activity when the CuO-TiO₂ nanocomposite is employed in such applications.
Field emission scanning electron microscopy and energy dispersive X-ray spectroscopy analysis
Figures 5(a) and 5(b) present the FESEM micrographs of the CuO-TiO₂ nanocomposite captured at magnifications of 200 kx and 400 kx, respectively. The images illustrate a highly agglomerated morphology, signifying the successful synthesis of the nanocomposite structure. The spherical CuO-TiO₂ nanocomposite appears densely packed, indicating strong interactions between the CuONPs and TiO₂NPs phases. The FESEM for CuO-TiO2 nanocomposite synthesized from the plant HS revealed an average size of 54.73 nm. The particle size distribution, as shown in the accompanying histogram, demonstrates relatively uniform sizes, reflecting the effectiveness of the synthesis parameters utilized during preparation. This observed morphology corresponds to the typical characteristics of CuO-TiO₂ nanocomposite, which are known for their enhanced photocatalytic performance due to an increased surface area and consistent particle distribution [40]. The particle size distribution, as illustrated in Figure 5(c), confirms the predominance of particles within a narrow range, with most particles falling within a specific size interval. This distribution reflects the controlled synthesis conditions, facilitated by the use of plant extract as a stabilizing, capping, and reducing agent. The histogram suggests that the synthesis method effectively minimizes particle size variations, which is critical for achieving consistent photocatalytic properties. The EDS spectrum in Figure 5(d) and the subsequent elemental composition table provide quantitative insights into the chemical composition of the nanocomposite. The prominent peaks of titanium (Ti, 43.65%) and copper (Cu, 21.18%) confirm the successful incorporation of both TiO₂NPs and CuONPs phases into the nanocomposite. Oxygen (O) constitutes 29.18% of the composition, confirming the presence of oxide phases. The trace amounts of magnesium (Mg, 0.17%) and carbon (C, 5.82%) are likely residuals from the plant extract and synthesis process [41]. The absence of silicon (Si) and calcium (Ca) further supports the purity of the synthesized material. The FESEM analysis reveals a well-defined nanostructured morphology with uniform particle size distribution, while the EDS analysis confirms the successful synthesis of a CuO-TiO₂ nanocomposite with a high degree of purity. The synergistic integration of CuONPs and TiO₂NPs phases, simplified by the HS extract, highlights the potential of this nanocomposite for photocatalytic applications, particularly in environmental remediation processes such as dye degradation.
Dynamic light scattering of CuO-TiO2 nanocomposites
The particle size distribution of CuO-TiO₂ nanocomposite, measured using DLS, was determined to be 490.40 ± 6.66 nm, with a PDI of 0.30 ± 0.02, as shown in Figure 6. This nanocomposite was synthesized from CuONPs and TiO₂NPs. The reasonably low PDI value of 0.30 ± 0.02 reflects good particle dispersion, indicating a stable suspension with minimal aggregation. The size measurements obtained through DLS represent the hydrodynamic diameter of the particles in solution, which accounts for both the particle core and the surrounding solvent layer, resulting in slightly larger particle size values compared to other measurement techniques focused solely on the core dimensions [42].
The multi-point BET analysis offers valuable insights into the surface characteristics and porosity of the CuO-TiO₂ nanocomposite synthesized using the Hibiscus sabdariffa (HS) plant extract. Figure 7(a) highlights the single-point surface area, measured at 17.95 m²/g at a relative pressure (P/P₀) of 0.29. This value represents the specific surface area of the material at this particular pressure. In contrast, Figure 7(b) reports a total BET surface area of 20.06 m²/g, calculated over a broader range of relative pressures, providing a cumulative measure of surface area based on N₂ adsorption. Moreover, the external surface area is determined to be 29.81 m²/g, reflecting a substantial contribution from external surface features alongside the microporous structure of the CuO-TiO₂ nanocomposite [43]. The nanocomposites demonstrated a BET surface area of 59.52 m²/g, suggesting a highly porous structure appropriate for photocatalysis. These variations emphasize the influence of the synthesis method and the use of HS extract on the material’s surface properties, which are critical for applications such as catalysis and adsorption, where the surface area directly impacts performance. Figure 7(c) shows the single-point adsorption total pore volume of pores smaller than 11.46 Å at P/P₀ = 0.010, measured at 0.002 cm³/g. This low pore volume within the sub-20 Å range indicates a limited fraction of micropores. The average pore diameter calculated using the BET method is 5.40 Å, characteristic of microporous structures (<20 Å). However, Figure 7(d) reveals a significantly larger average pore diameter of 100.64 Å, based on desorption data, indicative of mesopores or potentially macropores. This contrast highlights a broad pore size distribution in the CuO-TiO₂ nanocomposite [44]. The BET analysis indicates a hierarchical pore structure, characterized by the presence of both micropores and mesopores. Micropores contribute to enhanced surface interactions, improving adsorption and catalytic efficiency, while mesopores facilitate molecular transport and diffusion. This combination synergistically improves the material’s functionality, making it highly versatile for industrial applications such as adsorption, catalysis, and gas separation [45]. The measured BET surface area of the CuO-TiO₂ nanocomposite (20.06 m²/g) falls within the range typically reported for photocatalysts, which generally exhibit BET surface areas between 5 m²/g and 200 m²/g, depending on the synthesis method and material composition. Standard photocatalytic materials such as CuONPs often exhibit BET surface areas in the range of 10–100 m²/g, and TiO₂NPs in the range of 10–50 m²/g. Thus, the reported values support the standard results for photocatalytic materials, confirming their potential applicability for photocatalysis. The hierarchical porosity and sufficient surface area further validate its suitability for photocatalytic applications, potentially improving reaction kinetics and overall performance [46], [47]. Table 2 illustrates textural properties of the CuO–TiO₂ nanocomposite obtained from BET nitrogen adsorption–desorption analysis, including surface area, pore volume, and pore size distribution.
The PL spectrum of the CuO-TiO₂ nanocomposites in Figure 8 reveals distinct emission peaks, revealing the recombination dynamics of photo-generated charge carriers. The major peaks observed at approximately 400 nm and 800 nm are related to transitions within the material’s electronic structure [48]. Peak at ~400 nm, this peak links to the near-band-edge emission of TiO₂NPs, typically arising from the recombination of electron-hole pairs. Its intensity reflects the bandgap energy of TiO₂NPs in the composite. Peak at ~800 nm, this peak is likely associated with CuONPs and may be attributed to deep-level or defect-related emissions. The presence of this peak indicates the role of CuONPs in trapping charge carriers, which can suppress direct recombination and enhance the lifetime of charge carriers. The complete PL intensity provides insight into the charge carrier recombination rate. A reduced PL intensity, compared to pure TiO₂NPs or CuONPs, suggests improved charge separation in the composite material. This improvement is critical for enhancing photocatalytic activity, as it minimizes recombination losses and facilitates more efficient charge transfer to reactive sites [49]. The two peaks suggest an effective heterojunction between CuONPs and TiO₂NPs, promoting charge transfer and separation, which are advantageous for photocatalytic applications such as pollutant degradation.
The thermogravimetric and differential thermal analysis
Figure 9(a) presents the TGA curve for CuO-TiO₂ nanocomposites, temperature between 50 °C and 300 °C, showing a total weight loss of 5.91% as the temperature increases. The initial weight reduction is attributed to the evaporation of physically adsorbed moisture and other volatile organic compounds resulting from the green synthesis process. Following this, a further weight loss of 1.98% is observed between 301 °C and 800 °C, liable due to the breakdown of residual organics or decomposition of any remaining synthesis precursors. Beyond 800 °C, a further decline of approximately 3.53% is recorded, which eventually stabilizes, indicating the thermal resilience of the synthesized CuO-TiO₂ nanocomposites [50].
In Figure 9(b), the DTA curve highlights the rate of weight alteration with respect to temperature. Peaks at 217 °C in the DTA curve represent the highest rates of weight loss, signaling specific decomposition events. The appearance of multiple peaks implies several distinct degradation stages, likely due to the removal of different organic compounds from the synthesis or surface treatment processes. Cooperatively, these TGA and DTA results demonstrate the multi-step decomposition behavior typical of green-synthesized metal oxide nanocomposite. The final stabilized weight at elevated temperatures suggests the successful formation of CuO-TiO₂ nanocomposites, signifying the sample’s thermal stability and purity after the decomposition of organic residues [51].
Gas Chromatography- Mass Spectroscopy
The GC-MS chromatogram of HS extract in Figure 10 reveals prominent peaks at various RT notable peaks are observed around ~10 min, ~12 min, ~20 min, and ~30 min corresponding to diverse bioactive phytochemicals. These compounds were identified through their RT analysis, spectral comparison with established GC-MS libraries, and confirmation with published literature. The analysis underscores the richness of the extract’s phytochemical profile, which is mostly composed of fatty acids, phytosterols, aromatic compounds, triterpenoids, ketones, and esters. These bioactive constituents collectively contribute to the pharmacological relevance of HS, particularly in antioxidant, anti-inflammatory, antimicrobial, and lipid-regulatory applications [52].
1. Fatty Acids: The presence of hexadecanoic acid (palmitic acid), linoleic acid, and octadecanoic acid (stearic acid) is noteworthy. These essential fatty acids are well-documented for their anti-inflammatory, antioxidant, and lipid metabolism-regulating properties. Linoleic acid, a polyunsaturated fatty acid, is particularly significant in maintaining membrane fluidity and modulating inflammation pathways.
2. Phytosterols, the GC-MS analysis confirmed the occurrence of stigmasterol and beta-sitosterol, two structurally similar plant sterols. These compounds are recognized for their cholesterol-lowering effects through competitive inhibition of cholesterol absorption in the intestine, as well as their potent anti-inflammatory and antioxidant activities.
3. Aromatic Compounds, bioactive compounds such as 2,3-dihydrobenzofuran and 1,2-benzenedicarboxylic acid were identified. These aromatic compounds exhibit significant antimicrobial properties, inhibiting microbial growth by disrupting cellular integrity. Furthermore, they demonstrate antioxidant potential by scavenging free radicals, which helps mitigate oxidative stress.
4. Triterpenoids: the detection of squalene highlights the extract’s therapeutic value. Squalene, a bioactive triterpenoid, functions as a powerful antioxidant and is widely recognized for its anti-cancer properties. It also plays a role in skin protection by reducing damage caused by UV radiation and oxidative stress.
5. Ketones and Esters, compounds such as hexadecanoic acid methyl ester and 2-heptanone, further increase the pharmacological value of the extract. Hexadecanoic acid methyl ester has demonstrated antioxidant activity, while 2-heptanone is known for its antimicrobial and flavoring properties.
Table 3 summarizes the GC-MS analysis of the HS extract, which reveals a broad spectrum of bioactive compounds, including fatty acids, phytosterols, aromatic compounds, triterpenoids, and ketones/esters. These compounds are well-documented for their pharmacological properties, including antioxidants, anti-inflammatory, antimicrobial, and cholesterol-lowering effects. The results underscore the significant therapeutic potential of HS, suggesting its promising role in the pharmaceutical, nutraceutical, and functional food sectors. To further substantiate these bioactivities, additional in vitro and in vivo studies are recommended to explore their mechanisms of action and validate their therapeutic efficacy [53]
The photocatalytic degradation of methylene blue (MB) using the CuO–TiO₂ nanocomposite proceeds via the generation of reactive oxygen species (ROS) under ultraviolet (UV) irradiation. Upon exposure to UV light, both TiO₂ and CuO absorb energy, resulting in the excitation of electrons (e⁻) from the valence band (VB) to the conduction band (CB), leaving behind positively charged holes (h⁺) in the VB [67]. The formation of a heterojunction between TiO₂ and CuO enhances charge carrier separation and significantly reduces the rate of electron–hole recombination, thereby improving overall photocatalytic performance [68].
The photogenerated electrons reduce molecular oxygen (O₂) adsorbed on the catalyst surface into superoxide radicals (•O₂⁻), while the holes oxidize surface-bound water molecules or hydroxide ions to produce hydroxyl radicals (•OH) [69]. These ROS are highly reactive and responsible for attacking and decomposing MB dye molecules into smaller, less harmful end products such as CO₂ and H₂O [70]. The sequential photocatalytic steps can be described as follows:
1. CuO–TiO₂ + hν → e⁻ (CB) + h⁺ (VB)
2. e⁻ + O₂ → •O₂⁻
3. h⁺ + H₂O/OH⁻ → •OH
4. •O₂⁻ / •OH + MB → Degraded products (CO₂, H₂O, etc.)
The synergistic coupling between CuO and TiO₂ improves both light absorption and charge separation dynamics. This interaction, through the formation of a type-II heterojunction, extends the photoresponse and facilitates effective interfacial charge transfer, thus rendering the composite more active than the individual oxides [71]. The degradation of MB involves cleavage of the dye’s chromophoric groups, resulting in visible decolorization and subsequent transformation into environmentally benign substances or full mineralization into CO₂, H₂O, NH₃, and inorganic ions such as Cl⁻ and SO₄²⁻. The CuO–TiO₂ photocatalyst generates ROS, including hydroxyl radicals and superoxide anions, that disrupt the dye’s conjugated structures, leading to molecular breakdown [72], as schematically illustrated in Figure 11.
Intermediate degradation products, such as benzenesulfonic acid or aromatic amines, may be formed before complete mineralization. Therefore, the safety of treated water relies on the extent of mineralization achieved. Incomplete degradation may lead to the presence of toxic by-products, while changes in pH due to photocatalytic activity and the persistence of photocatalyst residues in treated water can further influence water [73], [74].
To confirm the complete degradation of MB and the safety of treated effluents, the following approaches are recommended:
• Total Organic Carbon (TOC) or High-Performance Liquid Chromatography (HPLC) to assess mineralization efficiency.
• Filtration or appropriate post-treatment techniques to remove residual nanocomposite.
• Ecotoxicological evaluations to ensure the absence of harmful effects in the final water output.
While decolorization indicates disruption of the dye’s chromophores, comprehensive analysis is essential to verify full mineralization and eliminate the possibility of hazardous intermediates [75].
Photocatalytic Kinetics and Optimum Conditions
The photocatalytic activity of the green-synthesized CuO–TiO₂ nanocomposite was assessed through the degradation of methylene blue (MB) under UV light. In this study, 10 mg of the nanocomposite was dispersed in 100 mL of a 20 mg/L MB solution, achieving approximately 81% degradation after 160 minutes of UV irradiation. Although no systematic optimization of parameters such as catalyst loading, pH, or initial dye concentration was performed, the selected experimental conditions were based on commonly reported effective ranges in the literature [76]. The high-rate constant (k) and strong correlation coefficient (R² > 0.98) indicate efficient photocatalytic activity. This performance is attributed to the synergistic interaction at the CuO–TiO₂ heterojunction, which enhances charge separation and suppresses electron–hole recombination, consistent with previous reports.
Scientific Significance of the Study
The use of HS flower extract as a green reductant and stabilizing agent offers a sustainable and environmentally friendly synthesis route, eliminating the need for hazardous chemicals. The heterojunction between CuONPs and TiO₂NPs not only broadens the optical absorption range but also promotes efficient charge carrier separation, thus improving the photocatalytic degradation efficiency [77]. The findings underscore the potential of the CuO–TiO₂ nanocomposites as an effective and low-cost material for environmental remediation, particularly in the treatment of dye-contaminated wastewater. CuO–TiO₂ nanocomposites have previously demonstrated high efficiency in the degradation of various dyes under visible light, owing to the formation of heterojunctions that facilitate charge separation and extend light absorption [78]. Moreover, the synthesis approach aligns with green chemistry principles, demonstrating scientific value through sustainable material development. Similar enhancements in photocatalytic performance have been observed in other oxide-based heterojunctions such as ZnO–TiO₂, which exhibit improved charge separation and degradation efficiency due to synergistic effects between the semiconductors ([79].
The photocatalytic degradation of MB dye using green-synthesized CuO–TiO₂ nanocomposites is demonstrated through a series of UV–Vis absorbance spectra in Figure 12(a), highlighting the time-dependent decline in MB concentration under UV irradiation. Figure 12(b) illustrates the corresponding degradation efficiency over time, while Figure 12(c) presents the pseudo-first-order kinetic plot of the degradation process. Collectively, these figures emphasize the high photocatalytic efficiency, stability, and kinetic behavior of the CuO–TiO₂ nanocomposites. In Figure 12(a), the UV–Vis spectra show the progression of MB degradation, with the initial absorbance at 0 minutes representing the maximum dye concentration. A significant reduction in peak intensity over time indicates effective photocatalytic activity. The nanocomposite achieved an 81% degradation efficiency within 160 minutes of UV exposure. This performance is attributed to enhanced light absorption and improved electron transport, resulting from the synergistic interaction between CuONPs and TiO₂NPs [80]. The integration of CuONPs into the TiO₂NPs matrix extends the absorption range from the UV to the visible spectrum, promoting greater electron–hole pair generation and efficient charge separation. These features enhance the interaction between the photocatalyst and dye molecules, thereby improving degradation efficiency [81]. Figure 12(b) further shows the photocatalytic efficiency of the CuO–TiO₂ nanocomposites across multiple cycles. A slight decline in efficiency after the first cycle may be due to surface fouling or partial deactivation of active sites. Nonetheless, the catalyst maintained stable performance in subsequent cycles, demonstrating its durability and reusability in photocatalytic applications [82]. Such stability is critical for practical implementation in wastewater treatment systems. Furthermore, the eco-friendly green synthesis of the CuO–TiO₂ nanocomposites aligns with sustainable production practices and suggests potential for cost-effective applications, although further investigation is needed to evaluate long-term usability and reusability [83]. Figure 12(c) presents a kinetic analysis based on the pseudo-first-order model, plotting ln(A/A₀) against time. The linearity of the plot, with a negative slope and a correlation coefficient (R²) of 0.93245 for MB, confirms that the degradation follows pseudo-first-order kinetics [84]. This indicates that the degradation rate is directly proportional to the dye concentration [85]. The consistent linear trend underscores the predictable and reliable photocatalytic performance of the CuO–TiO₂.
Table 4 shows photocatalytic degradation efficiencies of CuO-TiO2 nanocomposites synthesized with respect to various other synthesis methods and plant extracts.
LETHALITY ASSAY BRINE SHRIMP CYSTS
A progressive increase in lethality over 24, 48, and 72 hours is evident, as demonstrated in Figure 13(a–c), indicating a time-dependent toxicological response. This suggests that prolonged exposure to CuO-TiO₂ nanocomposites results in heightened toxicity to brine shrimp cysts, indicating cumulative or time-dependent toxic effects. The highest concentrations of CuO-TiO₂ nanocomposites consistently exhibited the greatest toxicity at all time points, with a steady decrease in the survival rate of brine shrimp as exposure duration increased. This trend underscores the importance of both nanocomposites concentration and exposure time in assessing the ecological and biological impact of CuO-TiO₂ nanocomposites. The prolonged lethality effect could be attributed to the combined properties of CuONPs and TiO₂NPs, which may enhance the oxidative stress on the organisms, leading to more pronounced toxic effects. Moreover, the findings highlight the necessity of carefully evaluating the long-term environmental risks associated with the use of such nanocomposites, particularly in aquatic ecosystems, where cumulative exposure could have detrimental consequences on biodiversity and food chain stability [88]. Figures 14(a) and (b) show the microscopic image of a control brine shrimp and a brine shrimp exposed to the synthesized nanocomposites, respectively.
CONCLUSION AND FUTURE DIRECTIONS
This study explored the green synthesis of CuO–TiO₂ nanocomposites using HS flower extract, aiming to develop a more environmentally benign approach to nanomaterial synthesis. The synthesis process yielded crystalline and thermally stable nanocomposites, as confirmed by structural and morphological characterizations. The nanocomposites demonstrated a photocatalytic degradation efficiency of 81% for MB under UV irradiation within 160 minutes, indicating their potential for application in organic dye removal from wastewater.
The enhanced photocatalytic activity is attributed to the synergistic interaction between CuONPs and TiO₂NPs, which may contribute to improved charge separation and surface reactivity. However, it is important to note that this conclusion is based on a single model dye (MB) under controlled laboratory conditions. Further tests with other pollutant classes and real wastewater matrices are required to validate broader applicability.
Toxicity assessment using brine shrimp indicated some level of biological impact, highlighting the necessity of further toxicological studies before environmental deployment. While the findings are promising, the absence of recyclability or reusability tests limits claims about the material’s long-term practical performance.
Future research should focus on
• Evaluating the nanocomposite’s photocatalytic performance against a wider range of pollutants, including persistent organic compounds and heavy metals.
• Exploring the material’s performance under solar irradiation to enhance sustainability.
• Investigating degradation mechanisms and identifying intermediate/by-products.
• Assessing the material’s environmental fate, long-term stability, and ecotoxicological profile under realistic environmental conditions.
• Scaling up the synthesis process and conducting pilot-scale studies in collaboration with industrial stakeholders.
In summary, while the current results establish the potential of HS-mediated CuO–TiO₂ nanocomposites for dye degradation, further comprehensive studies are required to substantiate their broader environmental and practical applications. This work provides a foundational step toward sustainable photocatalyst development, with a clear path for future validation and optimization.
The authors express their sincere appreciation to the Kurita Water Environment Foundation [23Pmy305] and UPM Grant 6380169 for their financial support. We acknowledge the support from the NANOTEDD research group of the Biophysics Laboratory at Universiti Putra Malaysia. We express our gratitude to Synchrotron Light for Experimental Science and Applications in the Middle East for the in-kind grant associated with the accepted proposal for MS/XPD & IR beamlines (Proposal # 20235204 - 20230152). We would like to express our gratitude to the Tertiary Education Trust Fund (TETFund) for supporting Abubakar’s PhD studies at UPM.
The authors confirm that there are no conflicts of interest that may have impacted on the research presented in this paper.
The principal contributions of the authors are outlined as follows: Che Azurahanim Che Abdullah has been instrumental in the conception and research design, secured research funding through the KWEF grant, and has actively participated in the critical revision of the manuscript, ensuring substantial intellectual content. Abubakar Meli played a crucial role in conducting experiments, gathering data, and analyzing and interpreting the findings related to the study. Mahmoud Abdellatief is engaged in characterization at SESAME utilizing MS/PXRD techniques and performing data analysis. Nazzatush Shimar Jamaludin focused on the design and analysis of photocatalytic systems. Che Azurahanim Che Abdullah contributed greatly to the completion and endorsement of the published version.
The data that support the findings of this study are available from the corresponding authors upon reasonable request.