Document Type : Original Research Paper
Graphical Abstract
Introduction
A vast field of science and engineering known as “nanotechnology” manipulates and investigates materials at the nanoscale to study them. The field of nanotechnology involves the investigation and synthesis of materials with sizes between 1 and 100 nm. Due to their extremely small size, these nanoparticles (NPs), the foundation of nanotechnology, have unique features. These characteristics diverge significantly from bulk material properties [1; 2]. Among the diverse array of NPs, metal NPs have attracted noteworthy interest due to their remarkable magnetic, optical, mechanical, and electronic characteristics, paving the way for an extensive range of uses in numerous scientific and technological fields[3]. Because the materials employed in other conventional procedures are expensive and hazardous, attention has been drawn to the eco-friendly and economical way to synthesize nanoparticles. But the most economical, time- and money-efficient, environmentally friendly, and physiologically safe approach is green synthesis[4].
Silver nanoparticles (AgNPs) have attracted significant attention in this field due to their special properties, such as photocatalytic activity. Due to their exceptional electrical, optical, and antibacterial qualities, silver nanoparticles (AgNPs) are well-known in nanotechnology [5; 6]. AgNPs also have a large ratio of surface area-to-volume and are frequently employed as catalysts in the photodegradation process[7]. On the other hand, traditional methods of producing AgNPs require harsh and hazardous chemicals, raising concerns about their detrimental environmental impacts. To pursue sustainable approaches, green synthesis methods for AgNPs have become a promising alternative. These methods use natural and environmentally friendly precursors to produce nanoparticles[2; 8]. Numerous phytocompounds found in plant extracts are used as capping and reducing agents during the synthesis of nanoparticles[9]. The primary phytocompounds that are accountable for the synthesis of AgNPs are flavonoids and antioxidant polyphenols. AgNPs are formed when silver ions are reduced from Ag+ to Ag. Additionally, flavonoids function as capping agents, stabilizing the size and shape of the formed nanoparticles during the synthesis process. Additionally, these phytocompounds tend to adsorb on nanoparticle surfaces[10; 11].
The plant extract concentration, temperature, PH, metal salt concentration, and reaction time all affect the rate, amount produced, and characteristics of the nanoparticles during the green synthesis of nanoparticles using plant extracts [12]. Various plant extracts, such as Lysiloma acapulcensis [13], Ocimum canum [14], Gymnema sylvestre leaf [15], Aerva lanata[16], Azadirachta indica [17], Benincasa hispida [18], Catharanthus roseus [19], Caesalpinia pulcherrima [20], Melissa officinalis [21], Pedalium murex [22], Parkia speciosa [23], Cotyledon orbiculata [24], Diospyros lotus [25], and Andean blackberry leaf [26], have been effectively reported regarding AgNPs biosynthesis. Green sea algae, remarkable organisms in the natural world, serve as a rich source of pectin. Pectin, a natural polysaccharide, serves as a stabilizing and reducing agent, offering a suitable replacement for harmful chemicals in AgNPs synthesis [27].
As industrialization progresses, there is increasing concern about the widespread discharge of dangerous materials into the environment. There are far more dyes, insecticides, phenols, and other organic pollutants with potentially hazardous consequences. Nitrophenols are among the most common contaminants found in wastewater [28]. Comparatively, methylene blue (MB), a cationic diazine dye, is extensively employed in various industrial applications. Practical methods are therefore currently required globally to remove these pollutants from industrial effluent [29]. Wastewaters containing organic pollutants have frequently been treated using chemical processes like oxidation and reduction, physical processes like adsorption, precipitation, reverse osmosis, and biological processes like aerobic and anaerobic intervention. One way to purify water is through photocatalytic degradation. Currently, biosynthesized nano-catalysts are commonly utilized to remove pollutants from water [30].
Despite previous studies on green synthesis of AgNPs, the use of pectin extracted from green sea algae for this purpose, particularly in the photocatalytic degradation of organic pollutants, remains a relatively under-investigated field, highlighting the need for further exploration. This study presents the following innovations:
• Utilizing pectin extracted from green sea algae for the synthesis of silver nanoparticles, which has been rarely investigated.
• Introducing a green, sustainable, and environmentally friendly method for AgNP production.
• Conducting a comprehensive structural, morphological, and physicochemical analysis of the synthesized nanoparticles.
• Evaluating the photocatalytic efficiency of the nanoparticles in degrading model organic pollutants such as 4-nitrophenol and methylene blue (MB) under light exposure.
• Developing an innovative approach with potential applications in water and wastewater treatment, clean energy production, and biomedical technologies.
Green algae are collected from the Caspian Sea. The Merck Company provided the necessary materials for the extraction process, including 96% ethanol, sodium hydroxide, hydrochloric acid (37%), and silver nitrate (AgNO3).
Several commonly used methods have also been employed to better understand and investigate nanoparticle properties, such as UV-Vis, XRD, FTIR, TEM, and SEM. UV-Vis spectral analysis was carried out using a Phystec-miniature UVS-2500 spectrophotometer. 1 nm resolution was obtained in the 190–800 nm range using a UV–visible absorption spectrophotometer. The Avatar Thermo Spectrophotometer system was used to record FT-IR spectra. The surface morphology and particle size were examined with a scanning electron microscope, the SEM FEI Quanta 200. Spectral analysis was utilized for the XRD (Philips PW 1730). The synthesized AgNPs’ amorphous nature is confirmed through XRD analysis within the angle range of 20°–80° and X-ray diffraction analysis.
Preparing Pectin from sea algae
Step 1: Collection and Initial Preparation of Sea Algae
• Fresh sea algae were collected from the Caspian Sea in northern Iran.
• The algae were first washed with tap water to remove surface dirt and impurities.
• They were then washed again with deionized water to eliminate any remaining salts and particles.
• The cleaned algae were air-dried at ambient temperature.
• After drying, the algae were cut into small pieces to facilitate the extraction process.
Step 2: Preparation of the Extraction Mixture
• 50 grams of dried and chopped algae were placed in a 250 mL glass Erlenmeyer flask.
• 180 mL of deionized water was added to the dried algae.
• HCl (hydrochloric acid) was added to adjust the pH of the solution to 2.
Step 3: Pectin Extraction Using Ultrasonication
• The Erlenmeyer flask containing the mixture was placed in an ultrasonic device (Parsonic 2600; Iran).
• The sonication process was carried out for 22 minutes at a temperature of 70°C.
• During sonication, ultrasonic waves disrupted the cell walls of the algae, releasing the pectin.
• After sonication, the Erlenmeyer flask was removed from the device and allowed to cool slightly.
• To precipitate the pectin, 96% ethanol was added to the extraction solution.
• The ratio of extraction solution to ethanol was 1:2.
• The mixture was left to rest at room temperature for 24 hours to allow complete precipitation of the pectin.
Filtration and Washing of Pectin
• After 24 hours, the solution was filtered through filter paper in a funnel to separate the precipitated pectin.
• The collected pectin was washed several times with 96% ethanol to remove impurities.
Step 6: Drying and Determining the Extraction Yield
• The precipitated pectin was dried in an oven at 60°C.
• After drying, the pectin was weighed to determine the amount extracted.
• From 50 grams of green sea algae, 12.53 grams of pure pectin were obtained.
Commonly, an AgNO3 aqueous solution and a pectin extract are utilized. The synthesis of nanoparticles happens at ambient temperature and completes in 30 minutes. In a glass Erlenmeyer flask, 90 mL of deionized water was combined with the required amount of AgNO3 to prepare a 0.005 mM solution. The solution was stirred using a magnetic stirrer until the AgNO3 was completely dissolved. Then, 10 g of pectin was added to the AgNO3 solution (90 mL). The flask was left at room temperature for 30 minutes, during which the color changed from colorless to dark brown, showing that silver nanoparticles were forming. The nanoparticles were then separated and washed by centrifugation, and then allowed to dry in a 60°C oven.
Photo-catalytic degradation of MB dye by AgNPs
The photodegradation experiment involves preparing solutions of MB at a specific concentration and AgNP suspensions with varying concentrations (20, 40, 60, 80, and 100 mg/L). Reaction mixtures are then prepared by combining a fixed volume of the MB solution (10 mL) with varying volumes of the AgNP suspensions, and the final volumes are adjusted with deionized water to ensure consistency across all samples. These mixtures are kept for two hours in the dark to achieve adsorption equilibrium, and then exposed to a light source. At specific time intervals of 5, 10, 15, and 20 minutes, aliquots are taken from each reaction mixture, and their absorbance is measured. A UV-Vis spectrophotometer was used at the characteristic wavelength of MB to calculate the MB degradation efficiency.
A quartz cell was filled with an aqueous solution of 4-nitrophenol (0.005 M, 1 mL) and NaBH4 (0.03 M, 1 mL). The reduction reaction was then started by adding 40 mg/L of the catalyst (convenient concentration). UV-Vis spectroscopy was used to monitor the reaction’s progress every 0–10 minutes. At 318 nm, 4-nitrophenol exhibits its most significant absorption peak. This peak shifts to 400 nm when NaBH4 is added because a phenolate ion is formed. Following the phenolate ion reduction, the 400 nm peak flattens, and the 300 nm peak of the amine emerges. An absorption chart was plotted against the concentration chart to detect the response rate[31].
The structure of pectin contains numerous -OH groups, as evidenced by the major peak in the 3200–3600 cm⁻¹ range. The characteristic peaks of pectin were observed at 3377, 1538, 1343, 1234, and 991 cm⁻¹, each corresponding to specific functional groups. The 3377 cm⁻¹ peak corresponds to the stretching vibrations of the O-H bond, indicative of hydroxyl groups in polysaccharides and absorbed water. The 1538 cm⁻¹ peak is associated with the C=O stretching vibrations in carboxylate (-COO⁻) groups, confirming the presence of ionized carboxyl groups in pectin. The 1343 cm⁻¹ peak corresponds to the bending vibrations of the C-O-H bond, typical of carboxylic groups in polysaccharides, while the 1234 cm⁻¹ peak represents C-O stretching vibrations in ester groups (-COOCH₃), indicating the presence of methoxy groups. Additionally, the 991 cm⁻¹ peak is attributed to the C-O-C stretching vibrations, confirming the glycosidic linkages within the pectin polysaccharide structure. This analysis highlights the presence of hydroxyl (-OH), carboxylate (-COO⁻), ester (-COOCH₃), and glycosidic (C-O-C) bonds, which define the complex polysaccharide nature of pectin [32; 33].
The FTIR spectrum in Fig. 1b corresponds to AgNPs synthesized using pectin, which acts as both a reducing and stabilizing agent. The observed shifts in peak positions and intensities compared to pure pectin confirm strong interactions between functional groups and silver nanoparticles. The broad peak at 3396.6 cm⁻¹ corresponds to O-H stretching vibrations, indicating the presence of hydroxyl (-OH) groups in pectin, which play a crucial role in reducing Ag⁺ to Ag⁰ and stabilizing the nanoparticles. The peak at 1744.8 cm⁻¹ is related to C=O stretching in ester (-COOR) groups, suggesting the interaction of pectin’s methyl esters with AgNPs. The 1649.3 cm⁻¹ peak, associated with C=O stretching in carboxylate (-COO⁻) groups, signifies the involvement of carboxyl functional groups in the stabilization and capping of AgNPs. Additionally, 1387.9 cm⁻¹ corresponds to C-H bending vibrations from the pectin polysaccharide backbone, while 1248.3 cm⁻¹ represents C-O stretching in ester (-COOCH₃) and ether (C-O-C) groups, further confirming their role in stabilizing the nanoparticles. The 1086.6 cm⁻¹ peak is attributed to C-O-C stretching vibrations, confirming the presence of glycosidic linkages in pectin, and the 829.4 cm⁻¹ peak is linked to out-of-plane C-H bending vibrations in sugar rings, suggesting interactions between pectin and silver nanoparticles. These findings confirm that pectin effectively acts as both a reducing and stabilizing agent in AgNPs synthesis, with hydroxyl (-OH) and carboxylate (-COO⁻) groups facilitating the reduction of Ag⁺, while ester (-COOCH₃) and glycosidic (C-O-C) bonds aid in stabilization, ensuring the successful green synthesis of AgNPs. [34; 35].
Figure 2 presents the UV-Vis spectra of silver nanoparticles (AgNPs) synthesized using pectin extracts. Upon adding the extract to the AgNO₃ solution, a visible color change from colorless to dark brown occurs. This color shift, indicative of AgNP synthesis, results from the collective oscillation of free conduction electrons caused by an electromagnetic field interacting with them, a phenomenon known as Surface Plasmon Resonance (SPR) excitation [36]. All extracts successfully produced AgNPs, as evidenced by the distinct absorbance peaks observed between 432 and 450 nm in Figure 2. The SPR peak at approximately 432–450 nm corresponds to the collective oscillation of conduction electrons in AgNPs when excited by light, serving as a key indicator of nanoparticle formation and confirming their presence in the colloidal solution. The position and intensity of the SPR peak are influenced by factors such as particle size, shape, and aggregation state. A peak within this range typically indicates the presence of small, spherical AgNPs, while broader or red-shifted peaks suggest particle aggregation or larger nanoparticles.
The natural biomolecules in pectin, including hydroxyl (-OH) and carboxyl (-COO⁻) groups, facilitate the reduction of Ag⁺ to AgNPs and stabilize them, preventing excessive aggregation. The smooth and symmetric SPR peak suggests that the nanoparticles are well-dispersed with minimal aggregation. Furthermore, the absence of peaks beyond 500 nm confirms that the nanoparticles remain monodisperse and stable, highlighting the efficient capping and stabilization role of pectin in AgNP synthesis [37-39]. This absorption range (400-450 nm) is consistent with previously reported SPR peaks for AgNPs. The presence of these peaks confirms the successful formation of AgNPs [40].
The green synthesis of AgNPs’ crystal structure was ascertained using the XRD method. The pattern of XRD for the current green synthetic AgNPs is shown in Fig. 3. Some Bragg reflections are found, which can be used to index the bands for AgNPs’ face-centered cubic (fcc) structures. These reflections have 2Ɵ values of 38.65, 45.31, 61.35, and 77.12, respectively, corresponding to the sets of lattice planes (111), (200), (220), and (311). The (111) plane has more intensity than the other planes. JCPDS data card no. 96-900-8460 provided confirmation of the values of the diffraction peak and lattice constant. When the diffraction peaks are at half-maximum, to find the average crystallite size throughout the breadth, the Debye-Scherrer equation is applied [41].

β (in radians) represents the full width at half maximum (FWHM) of the diffraction peak in the Debye-Scherrer equation. The X-ray wavelength (1.54056 Å) is represented by λ, whereas D represents grain size. Using XRD measurements, the size of the crystallites was 12 ± 2.3 nm. AgNPs synthesized using the green method undoubtedly exhibit a nanocrystalline nature, as evidenced by unique structural peaks in the XRD patterns. These XRD patterns are consistent with previous studies of AgNPs produced using environmentally friendly processes [42-44].
Silver nanoparticles (AgNPs) were characterized using transmission electron microscopy (TEM). TEM is one of the most advanced imaging tools for determining the size, shape, and morphology of nanoparticles [45]. TEM images of the synthesized products confirm the presence of silver nanoparticles as dispersed dark spots against a lighter background. These images, captured within a range of 10 and 50 nm, indicate that the average size of the nanoparticles is 13 nm, with a noticeable size distribution.
While confirming their colloidal nature solely through TEM images is challenging, the appropriate dispersion and lack of severe aggregation suggest potential stabilization, likely due to residual organic matter such as pectin. The slightly hazy regions around some nanoparticles indicate the presence of these residual organic materials, which may influence their stability and properties. Additionally, the images reveal a wide dispersion and some degree of irregularity in the shape of the spherical nanoparticles.
To better examine the size distribution, a histogram was plotted, showing that most nanoparticles fall within the 13 nm range. This relatively broad distribution suggests variations in particle size, which align with TEM observations. These findings indicate that the nanoparticle system is well-dispersed and likely stabilized by organic matter.
Using FE-SEM analysis, morphology, surface homogeneity, and particle size may all be examined. Fig. 5 shows microscopy pictures of manufactured AgNPs at various concentrations of silver precursor. According to FE-SEM analyses, the nanoparticles’ typical diameters range from 32 to 100 nm, and their surface shape is spherical. FE-SEM images show that the nanoparticles are homogeneous and do not show significant aggregation.
Methylene blue dye photocatalytic degradation by AgNPs
The ability of metal nanoparticles to catalyze processes that would not otherwise be possible is one of their primary uses. The catalytic activity of nanoparticles is strongly influenced by their composition, size, and shape. Higher catalytic activity is generally indicated by a larger surface-to-volume ratio [46]. It is commonly known that during the dye reduction and removal process, AgNPs exhibit enhanced catalytic activity. The textile industry has recently seen a rise in the use of MB, a heterocyclic aromatic dye. The process above produced AgNPs, which were then utilized as a catalyst by NaBH4 to reduce MB.
A spectrophotometer was used to evaluate the AgNPs’ photocatalytic efficacy on the MB dye. In its oxidized condition, MB is blue; however, when reduced to MB, it becomes colorless. To investigate the photocatalytic effect of AgNPs on MB degradation, solutions containing a constant concentration of MB and varying concentrations of AgNPs (20, 40, 60, 80, and 100 mg/L) were used. After 25 minutes, the intensity of the absorption spectra for every solution was determined using UV-Vis spectroscopy. Figure 6a displays the UV-Vis absorption spectra of MB reduction without a catalyst (AgNPs). The UV-Vis absorption spectra of MB reduction with increasing concentrations of the synthesized catalyst are displayed in Fig. 6b. It was found from the data that as the AgNP concentration rises, MB absorption strength falls. Because a higher concentration of AgNPs provides more accessible and active sites on the catalyst’s surface, leading to an increase in hydroxyl radicals involved in the process. The absorption maxima of MB in an aqueous solution are often observed at 663 nm due to the π/π* and n/π* transitions[47]. The highest absorption band at 663 nm will diminish as the catalytic degradation proceeds; in comparison, a new band with a maximum of 432 nm will simultaneously develop and become more intense with time. Notably, the reduction of MB was completed in just 10 minutes in the presence of 20 mg/L of AgNPs.
A comparison of our findings with previous data on the duration required to attain 100% MB color reduction using AgNPs derived from a plant extract is shown in Table 1. AgNPs assist in the catalytic breakdown of MB, with a potential mechanism described by the Langmuir-Hinshelwood model[48]. Here, NaBH4 acts as a supply of hydrogen and an electron donor. It serves as an intermediary to transport electrons between the BH-4 ion and the MB due to its high damaging potential (-1.8 V vs. NHE) [49]. Instantaneous electron and hydrogen transfer occurs when NaBH4 is added to a solution containing AgNPs and MB. This occurs due to the BH4− ion from the MB and NaBH4 molecules adhering to the AgNPs’ surface. The colorless degraded by-product that results from diffusion between adsorbed molecules desorbs. AgNPs’ wide surface area may provide more catalytic sites for the breakdown of MB. These results show that adding AgNPs in the right amount increases the efficiency of the MB reduction reaction. These findings imply that the colloidal AgNPs produced serve as an efficient “green catalyst,” mediating electron transport during the reduction of MB. As a green catalyst, AgNPs act as electron transfer mediators, facilitating the movement of electrons from BH₄⁻ to MB, leading to its reduction into a colorless product. The high surface area of AgNPs enhances contact between reactant molecules, increasing catalytic efficiency. This process occurs without toxic chemical additives, making AgNPs an eco-friendly alternative to traditional chemical catalysts. Additionally, optimizing the amount of AgNPs is crucial, as an inadequate concentration may lead to a slow reaction, while an excessive amount might cause nanoparticle aggregation, reducing the available catalytic sites. Therefore, the efficient electron transfer, high catalytic activity, and eco-friendly nature of AgNPs confirm their role as a promising green catalyst for the degradation of organic pollutants like MB.
Catalytic activities of AgNPs in the 4-nitrophenol
Industries release combinations of phenol and nitroaromatic chemicals that are highly harmful to human health [53; 54]. Nitrophenolic compounds and their derivatives are specifically produced during the production of herbicides, insect repellents, and insecticides [55]. The 4-NP must be transformed into valuable compounds like 4-aminophenol (4-AP) to reduce its toxicity. In this work, 4-NP was catalytically reduced to 4-AP using green synthetic AgNPs. Green synthesis AgNPs were utilized as a catalyst to remove the kinetic barrier that slowed the transfer of electrons from the donor (BH4-) to the acceptor, 4-NP. As shown in Fig. 7, a strong peak that 4-NP displayed at 317 nm was shifted to 400 nm using NaBH4, and the absorbance at 400 nm was used to measure the reduction process. At 400 nm, a steady decline in absorbance was seen, and after adding the reaction mix containing the biosynthesized AgNPs. Similarly, during 5 minutes at 298 nm, the peak intensity increased. The complete reduction of 4-NP dye, evidenced by the disappearance of its yellow color, was achieved within 15 minutes under UV light irradiation. This suggests the successful 4-NP to 4-AP conversion. The proposed reaction mechanism for this photocatalytic reduction involves four key steps: (Ι) Hydrogen from the BH4- ion is adsorbed onto the surface of the AgNPs. (ΙΙ) The surface of the AgNPs absorbs the 4-NP dye molecules. (ΙΙΙ) As a bridge, AgNPs help electrons move from the donor, the BH-4ion, to the acceptor, the 4-NP molecule. (
) The reduced 4-AP desorbs from the AgNPs surface (Scheme 1)[56]. The reaction time for 4-NP degradation has been compared with previous studies (Table 2).
The Reusability and Catalytic Efficiency of AgNPs in the Degradation of MB and 4-NP
To assess the reusability of AgNPs in the degradation of MB and 4-NP, multiple reaction cycles should be conducted to evaluate the catalytic performance of these nanoparticles in both processes. After each cycle, the AgNPs can be separated from the solution and reused in a new reaction mixture. The catalytic efficiency is determined by measuring the rate of color reduction and the color changes in the solutions. A decline in catalytic efficiency, accompanied by a slower reaction rate over successive cycles, suggests a reduction in the catalyst’s effectiveness.
The results from the table show that AgNPs reduce MB and 4-NP at high speed and excellent efficiency in the first cycle. However, as the number of cycles increases, both the rate of color reduction and the time required for complete reduction of both pollutants increase. In cycles 2 and 3, a slight decrease in catalytic efficiency is observed, indicating a gradual reduction in the effectiveness of AgNPs. In cycles 4 and 5, a significant decrease in catalytic efficiency leads to the loss of catalytic activity. This reduction in performance could be due to nanoparticle aggregation, structural degradation, or leaching of silver ions into the solution, which negatively impacts the efficiency and stability of the catalyst.
This study explored the potential of pectin extracted from algae for the green synthesis of AgNPs. The FT-IR analysis confirmed successful pectin extraction. The generated AgNPs had a crystalline structure and spherical morphology, as determined by UV-Vis, FT-IR, FE-SEM, XRD, and TEM analyses. This eco-friendly synthesis approach offers advantages like scalability and cost-effectiveness. The synthesized Ag-NPs demonstrated remarkable efficiency as a photocatalyst in degrading MB and as a catalyst in reducing 4-NP. Key advantages of these AgNPs include easy separation, high catalytic efficiency, excellent stability, and reusability without significant activity loss. These results indicate that these nanoparticles can be applied in water and wastewater treatment to eliminate recalcitrant organic pollutants.
The scalability limitations require further investigation for industrial-scale applications, and the impact of these nanoparticles under different environmental conditions and temperatures should also be evaluated. Additionally, the efficiency of silver nanoparticles in the presence of other pollutants and their ability to remove combined pollutants should be studied. Furthermore, assessing their long-term stability and environmental impacts in industrial and environmental applications is crucial. These issues can provide the basis for future research on the use of silver nanoparticles as a green catalyst in water and wastewater treatment and other industrial applications.
The authors declare no conflict of interest.