Document Type : Original Research Paper
Graphical Abstract
INTRODUCTION
Over the past decade, nanotechnology has gained immense attention from researchers worldwide due to its potential to revolutionize various scientific and industrial fields [1,2]. Among the different classes of nanomaterials, metal oxide nanoparticles (NPs) have emerged as particularly promising owing to their unique chemical and physical properties, cost-effectiveness, controlled grain size, and high stability [3,4]. Zinc oxide nanoparticles (ZnO NPs), in particular, have garnered significant interest for their remarkable biocompatibility, environmentally friendly nature, low toxicity, and simplicity of synthesis. Additionally, ZnO NPs exhibit high exciton binding energy and versatility in applications, making them indispensable in areas such as solar cells, gas sensors, ceramics, catalysts, cosmetics, and varistors [5-8]. Numerous methods have been explored for the synthesis of ZnO NPs, including sol-gel [9], solvothermal [10], hydrothermal [11], laser ablation [12], and the polyol process [13]. Among these, the polyol method stands out due to its simplicity, cost-effectiveness, and ability to produce nanoparticles with excellent crystallinity and controlled morphology [14]. The method typically involves the reduction of metal precursors in a polyol solvent, such as ethylene glycol or polyethylene glycol, which also acts as a stabilizing agent to minimize particle agglomeration and regulate growth [15,16]. The modified polyol method builds upon this approach by incorporating additives, such as surfactants or natural extracts, to further control nanoparticle size, shape, and properties [17].
The green synthesis approach signifies the use of plants with mild reaction conditions in the synthesis of nanoparticles and has gained traction due to their eco-friendly nature and alignment with sustainable practices [18-20]. Literature reported that Zn salt precursor and plant extract are mixed under constant stirring to undergo a hydrolysis reaction in which Zn²⁺ ions turn into zinc oxide nanoparticles [21]. Under such conditions, using various Zn precursors, along with plant extracts and controlling reaction parameters (usually time and temperature), ZnO nanoparticles of numerous sizes and morphologies can be obtained [22]. The diverse range of compounds found in plant extracts, including polysaccharides, alkaloids, steroids, flavonoids, tannins, saponins, glycosides, phenolics, proteins, peptides, and vitamins, serve dual roles as both reducing and capping agents for the green synthesis of nanoparticles, aligning with the inherent biological composition of these extracts [23].
Considering this, our research explores the synthesis of ZnO-NPs through modified polyol synthesis, employing Sapindus mukorossi plant extract in combination with ethylene glycol and PEG-4000 as reducing and stabilizing agents. This novel approach, utilizing ethylene glycol, soapnut extract, and PEG-4000, offers a unique, efficient, and previously unreported method, marking a significant advancement in nanoparticle synthesis. This research bridges the gap between traditional nanoparticle synthesis methods and environmentally friendly approaches utilizing natural resources.
Despite the advances in ZnO NP synthesis, challenges remain in achieving a balance between efficient, scalable production and environmental sustainability. To address these gaps, our research integrates the advantages of the polyol method with the principles of green chemistry, using Sapindus mukorossi extract and PEG-4000. The inclusion of high-molecular-weight PEG ensures enhanced reducing activity and nanoparticle stability, while the plant extract contributes to the green synthesis framework. This work not only improves nanoparticle quality and yield but also demonstrates the potential for scalable, sustainable production, addressing critical needs in nanotechnology and environmental science.
MATERIALS AND METHODS
The ACS grade chemicals zinc acetate dihydrate [Zn(CH3COO)2.2H2O], ethylene glycol Reag. USP grade and polyethylene glycol-4000 (PEG-4000) Reag. USP grades are procured from Merk India. The fruits of Sapindus mukorossi (reetha) were collected directly from trees in Ranikhet, Almora, Uttarakhand, India. Distilled water and deionized water having conductivity less than 1 μScm-1 at 25 ℃ were used throughout the experiment for preparing solutions and washing purposes.
Preparation of ethylene glycol extract of Sapindus mukorossi (reetha)
The collected fruits were washed three times with distilled water and then dried in sunlight. The peel was separated from the seeds by cutting the fruit. The peel portion was used to extract the plant surfactant. The peel material was crushed in a mortar to make smaller pieces and then finely powdered. 10 g of soapnut powder was placed in 100 mL of ethylene glycol (EG) in a conical flask and left undisturbed for a week. After 7 days, the solution was decanted and stored at room temperature for further use in nanoparticle synthesis.
Synthesis of ZnO Nanoparticles
0.1M Zn(CH3COOH)2·2H2O was dissolved in 45 mL of ethylene glycol and 5 mL ethylene glycol extract of Sapindus mukorossi (reetha). Then the solution was heated at 140 oC for 30 min under continuous magnetic stirring. The precursor solution was then kept at room temperature for 15 min. Subsequently, at room temperature, 0.1 g of polyethylene glycol (PEG-4000) was added to the solution and it was further heated at 140 oC for 45 min with continuous magnetic stirring. The mixture was cooled to room temperature, and the obtained product was washed several times with a mixture of acetone and water. Finally, the product was washed with water and ethanol, followed by centrifugation at 3700 rpm for 15 min to remove excess precursor. The collected final product was dried in a vacuum oven at 75-85 oC for 12 h to obtain zinc oxide nanoparticles in powdered form.
Characterization
The structure, optical properties, and morphology of the nanoparticles were characterized using various techniques: high-resolution transmission electron microscopy (HRTEM) - Model no. Tecnai G2 S-TWIN (FEI), UV-Vis spectrometer - Model Perkin Elmer Lambda 15, scanning electron microscopy (SEM) - Nova Nano FE-SEM 450 (FEI), Fourier Transform Infrared spectroscopy (FTIR) - Model Perkin Elmer Spectrum RX1 FTIR Spectrometer, X-ray diffraction (XRD) - Philips X’pert MPD system, and energy dispersive X-ray (EDX) - Thermo Scientific.
Antimicrobial Activity
The antibacterial and antifungal activity of synthesized ZnO NPs were analyzed with Gram-negative (Escherichia coli, MTCC- 452) and Gram-positive (Staphylococcus aureus, MTCC-96) bacterial strains and C. albicans (MTCC- 854), A. niger (MTCC-281) respectively by following Zone Inhibition Method (Kirby-Bauer method). The MHA (for antibacterial analysis; Mueller-Hilton Agar (MHA-SRL Chem- 24756)), SDA (for C. albicans; Sabouraud dextrose agar –SDA (SRL Chem, Cat no.- 19427)) and PDA (Potato Dextrose Agar (PDA - SRL Chem, Cat no.- 35208) for A. niger) plates were inoculated by spreading with 100 µL of Bacterial culture, E. coli and S. aureus (adjusted to 0.5 McFarland Unit - Approx cell density (1.5 X 108 CFU/mL) and followed by placing the discs containing 10 µL of different concentration (0 to 100 mg/mL). 10 % of the sample was taken and serially diluted to achieve the required amount to be loaded on the disc. One disc in each plate was loaded with solvent alone which served as vehicle control and the Ciprofloxacin (SRL Chem-78079) disc (10 µg) was taken as a positive control in case of antibacterial analysis and Amphotericin B (Amphocare) disc (50 µg) were taken as a positive control for antifungal analysis. The plates were incubated (Basil Scientific Corp. India- Incubator) at 37 oC for 24 h.
RESULTS AND DISCUSSION
XRD Analysis
X-ray diffraction (XRD) analysis of the nanoparticles elucidated their crystalline structure, providing insights into their composition and crystallographic properties. This technique is crucial for determining the phase purity and crystallinity of the synthesized nanoparticles. X-ray powder diffraction (XRD) studies were carried out using an X-ray diffractometer with Cu Kα radiation (λ=1.54Å). The X-ray wavelength was 0.15418 nm, and the data were recorded in the range of 5°-80°. X-ray diffraction patterns shown in Fig. 1 and sharp peaks indicate that the obtained ultra-fine particles are in good crystallinity. The prominent peaks observed at 2θ values of 31.9°, 34.5°, 36.3°, 47.6°, 56.7°, 62.9°, 66.5°, 68.0°, and 69.2° correspond to the lattice planes of (100), (002), (101), (102), (110), (103), (200), (112), and (201) respectively, which are indicative of the hexagonal wurtzite crystalline structure of ZnO nanoparticles according to JCPDS database card number [01-070-2551] [24,25].
The crystallite size of nanoparticles was calculated using the Debye-Scherrer formula.
Were λ is the wavelength of the X-ray source (0.1541 nm), β is the full width at half maximum (FWHM) in radians and θ is Bragg׳s diffraction angle. The average crystallite size of the prepared ZnO NPs was found to be 16 nm.
SEM-EDX analysis
The morphology of the ZnO nanoparticles (NPs) was investigated using scanning electron microscopy (SEM), as shown in Fig. 2, to visualize their size and shape. SEM is a powerful imaging technique that provides high-resolution, three-dimensional images of the surface morphology and topography of nanoscale materials, including nanocomposites. In SEM images, ZnO nanoparticles typically appear as thin, flakes (nanoflakes) arranged in various orientations and are aggregated into large agglomerates, showcasing the controlled synthesis of the material. Earlier literature has proven that the addition of PEG-4000 to ZnO crystals plays an important role in the development of nanoparticle morphology [26]. Furthermore, SEM imaging can be coupled with other analytical techniques, such as energy-dispersive X-ray spectroscopy (EDX), to provide compositional information about the flaky nanoparticles. This enables researchers to determine the elemental composition and chemical composition of the nanoparticles, as well as investigate any dopants or impurities present. The EDX spectrum confirmed the presence of zinc and oxygen peaks only in the synthesized ZnO NPs, indicating their purity (shown in Fig. 3). The atomic compositions for zinc (Zn) and oxygen (O) were found to be 67.44% and 32.56%, respectively, while the mass compositions for zinc (Zn) and oxygen (O) were 57.78% and 14.47%, respectively, in the synthesized ZnO NPs.
TEM analysis
TEM images of synthesized nanoparticles along with the SAED pattern are shown in Fig. 4(a, b). The particle size and morphological characteristics of the zinc oxide nanostructure were examined using transmission electron microscopy (TEM). TEM images revealed that the nanoparticle size ranges between 15 nm to 35 nm, with the average size of the ZnO nanoparticles being 21 nm, which correlates well with the size calculated from XRD analysis, confirming the excellent crystallinity of the ZnO nanoparticles. Selected Area Electron Diffraction (SAED) analysis further confirmed the presence of uniform size, shape, and phase purity, along with clear morphology and crystallinity. The crystalline nature of the synthesized ZnO nanoparticles was confirmed by SAED, which showed intermittent dots on the concentric circles, as depicted in Fig. 4(c).
The size of nanoparticles has a significant impact on the overall properties of materials, making it crucial to study the evolution of nanoparticle size, especially in semiconducting materials. UV-visible absorption spectroscopy is a commonly used technique for investigating the optical properties of nanoscale particles. Fig. 5(a) displays the absorption spectrum of ZnO NPs, showing a prominent absorption band around 360 nm, which is in good agreement with the previously reported data [27]. This absorption is attributed to the direct bandgap transition characteristic of ZnO, where electrons are excited from the valence band to the conduction band.
The bandgap energy of ZnO nanoparticles can be adjusted by manipulating their dimensions, structure, and form. When the nanoparticles are smaller, their bandgap energy increases due to quantum confinement effects [28]. Consequently, smaller nanoparticles feature a wider bandgap, resulting in improved UV absorption and optical characteristics. The Tauc’s plot (Fig. 5(b)) is a common method used to estimate the band gap of semiconductor nanoparticles according to the following equation;
αhν = A(hv − Eg)n
where α is the absorption coefficient, h is the photon energy, and Eg is the band-gap for direct transitions (n=1/2). For direct band gap materials like ZnO nanoparticles, the plot typically shows a linear region at higher photon energies. Extrapolating this linear portion to the x-axis yields the band gap energy (Eg), which represents the energy required to promote an electron from the valence band to the conduction band. The calculated direct band gap (Eg) for ZnO NPs was 4.7 eV [29].
FTIR Analysis
FTIR serves as a confirmatory technique for nanoparticle formation, providing insight into the vibrational and rotational modes of molecules, thereby aiding in the identification of functionality and stabilization of ZnO NPs. The FTIR spectra of ZnO nanoparticles were recorded using the KBr pellet method. Fig. 6 displays the FTIR spectrum of ZnO NPs. The peaks below 1000 cm−1, known as the fingerprint region, represent the intrinsic adsorption bands of metal oxides. The absorption band of ZnO appears in the range of 800 - 400 cm−1 [30,31]. FTIR spectrum of the saponin extract displayed broad bands at 3400 cm−1 for CH2 and hydroxyl groups this peak resembles those of saponin as reported in the literature [32-33]. The absorption band around 1384 cm-1 is designated to the bending vibration of -CH3 stretching [34].
Antimicrobial activity
A qualitative agar well diffusion test was conducted to evaluate the antimicrobial properties of ZnO NPs against Gram-positive bacteria (S. aureus), Gram-negative bacteria (E. coli); fungi C. albicans, and A. niger. The growth inhibitory effect of ZnO NPs was observed by the formation of clear zones on the MHA plates (Fig. 7). A larger zone of inhibition indicated higher sensitivity of the test organism to the nanoparticle, thus suggesting greater effectiveness of the nanoparticles. Table 1 presents the inhibition zones (in mm) observed around the nanoparticles and positive controls. The zone of inhibition is maximum at 500 μg for all strains. In this study, the nanoparticles were found to be most effective against S. aureus. The antimicrobial activity of ZnO NPs is attributed to the release of reactive oxygen species (ROS), including hydrogen peroxide (H2O2), hydroxyl radicals (•OH), and peroxide ions (O22−), from the surface of ZnO [35]. These ROS induce oxidative stress by damaging cellular proteins, membranes, and DNA. Upon contact with bacterial cells, ROS disrupts the microenvironment, causing damage and disorganization in bacterial cells, and releases antimicrobial ions (Zn2+) inside the cells, leading to toxicity. These ions can impair the cell membrane and penetrate the intracellular space [36, 37].
CONCLUSIONS
The comprehensive analysis of ZnO nanoparticles synthesized in this study highlights their significant potential in various applications. XRD analysis confirmed the hexagonal wurtzite crystalline structure of the ZnO nanoparticles with a crystalline size of 20 nm, aligning well with previous studies. The calculated direct band gap (Eg) of 4.7 eV indicates a slight enhancement compared to commonly reported values for ZnO NPs (approximately 3.3–3.7 eV), suggesting the influence of synthesis conditions on electronic properties. TEM analysis corroborated the XRD results, showing an average particle size of 21 nm, demonstrating good agreement between different characterization techniques. The synthesis parity and material integrity were further validated using FTIR, UV-Vis, XRD, and SEM-EDX, with EDX elemental analysis confirming the absence of impurities, which is crucial for biomedical and industrial applications. Morphological analysis through SEM revealed the formation of flake-like structures, which could be advantageous in enhancing surface area and reactivity. ZnO nanoparticles exhibited excellent antibacterial activity against both Gram-positive (S. aureus) and Gram-negative (E. coli) bacteria, with inhibition zones ranging from 12.67 mm to 18.33 mm. Additionally, the antifungal activity against C. albicans and A. niger demonstrated inhibition zones between 1.66 mm and 10.87 mm, indicating the broad-spectrum antimicrobial efficacy of the synthesized ZnO NPs. These results not only validate the effectiveness of the modified polyol synthesis method but also highlight its superiority in achieving bioactive nanoparticles with enhanced properties compared to conventional methods. The quantitative results of this study underscore the significance of employing a green and modified polyol method, leveraging Sapindus mukorossi extract and PEG-4000 for sustainable nanoparticle production. Compared to previous works, the synthesized ZnO NPs exhibit competitive or superior antibacterial and antifungal performance, emphasizing their potential as antimicrobial agents. These findings pave the way for the application of ZnO nanoparticles in biomedical fields, particularly in developing novel antimicrobial coatings, drug delivery systems, and other health-related technologies. Future studies should explore their scalability and functionality in real-world applications to further validate their practicality and commercial potential.
ACKNOWLEDGEMENTS
The authors express their gratitude to the Malaviya National Institute of Technology Jaipur and Aaakar Biotech Private Limited in Lucknow, India, for providing instrumental facilities. R.K. is thankful to the University Grants Commission, New Delhi, India, for the award of the Senior Research Fellowship. They also appreciate the valuable suggestions from Prof. Raj N. Mehrotra, Former Professor and Head of the Department of Chemistry at Jodhpur University.
Conflict of Interest
The authors declare that they have no conflict of interest related to the publication of this article.