1 Manonmaniam Sundaranar University, Abishekapatti, Tirunelveli 627 012, Tamil Nadu, India
2 Department of Physics, Pioneer Kumaraswamy College, Tamilnadu – 629003, India.
3 Department of Electronics and Communication Engineering, R.V.R. & J.C. College of Engineering, Andhra Pradesh - 522019, India
4 Department of Physics, Arunachala College of Engineering for Women, Tamilnadu-629203, India.
Abstract
Doping transition metals have great potential to enhance the optical and magnetic properties. This work described the synthesis of pure and FexZr 1-x O2 (x = 0.04, 0.08, and 0.12 mol %) nanoparticles, structural, magnetic, photocatalytic, and anti-microbial properties.  According to the results, Fe doping reduced the crystallite size from 29.74 to 7.88 nm. Smaller particles have a higher surface area-to-volume ratio, which can enhance their reactivity. UV-visible spectra, the produced un-doped, and Fe-doped zirconia nanoparticles have a comprehensive band-gap material ranging between 4.6 and 1.6 eV. A smaller band gap allows nanoparticles to absorb light more efficiently which enhances the photocatalytic activity. The diffraction pattern of pure and Iron-doped ZrO2 nanoparticles reveals a tetragonal crystalline phase. The retention of the tetragonal crystalline structure upon doping, despite introducing Fe3+, highlights a unique stability in the material. The SEM micrograph confirms the Pure ZrO2 nanoparticles have a rod-shaped morphology and spherical mixture of spherical and needle-shaped morphology for iron-doped zirconia with various concentrations. The hysteresis loop for pristine zirconia exhibits perfect Ferromagnetism at Room Temperature (RTFM), whereas iron-doped zirconia exhibits superparamagnetic behavior, according to a VSM investigation which offers several advantages in fields like medicine, and environmental remediation In addition, iron doping improves zirconia’s anti-microbial properties.

Graphical Abstract

The Impact of Fe-doped Nano Zirconia for the Reformation of the Photoreaction Rate and Materializing Microorganism Resistance
Keywords

Introduction

Synthesis of ceramic particles has attracted great attention owing to its properties such as good reaction ability, best homogeneity, and sinterability state[1,2]. Nano zirconia-based ceramics plays an important role due to its potential applications such as photocatalysis, and antimicrobial activity. Crystallite size and phase transformation are important parameters to determine the properties of zirconia nanoparticles. Normally pristine zirconium oxide nanoparticles exhibit three different crystal structures namely cubic, tetragonal, and monoclinic [3]. It is necessary to understand the correlation between crystal phase and crystallite size to enhance the performance of high surface area catalysts and nano-based devices[4].

Photocatalytic degradation through the Advanced Oxidation Process (AOP) is used in the degradation of hazardous materials like Methylene Blue (MB) dye. The hydroxyl radicals that are produced by AOPs are more capable of the degradation of chemical compounds due to the high electrochemical oxidation potential [23,24]. The Photocatalytic property of ZrO2 can be enhanced by doping it with metals or nonmetals or coupling it with semiconductors with narrower band gaps, which could prevent electron-hole recombination [5,6]. The photocatalytic activity of ZrO2 is affected by many parameters, including phase purity, crystallite size, dopant nature, and manufacturing method. Due to its moderate electron structure, Fe is an ideal choice for tuning the bandgap and improving the photocatalytic efficiency of ZrO2 among several metal elements [7]. According to scientific literature, Fe-doped ZrO2 has higher photocatalytic activity and a narrower bandgap than pure ZrO2. However, Fe-doped ZrO2’s visible-light photocatalytic performance is limited, and extensive information on the influence of Fe doping on the crystal structure and electronic structure of ZrO2 is lacking. Nanostructured materials can also be used in biomedical applications.

The synthesis technique and the nanoparticle size have crucial roles in enhancing features such as magnetic ordering temperature or Neel temperature, coercivity, magnetization, and magnetic moments, among others. The effect of photocatalytic and anti-microbial activities on the synthesis of Fe-doped Zirconia nanoparticles using the co-precipitation process is explored in this paper. The use of co-precipitation method used in this research for synthesizing Fe3+ doped ZrO2 nanoparticles is notable for its simplicity and effectiveness in producing materials with enhanced properties, setting it apart from more traditional synthesis techniques. The remarkable reduction of the bandgap in this method is a groundbreaking finding, showcasing how Fe doping creates new impurity energy levels that enhance light absorption, which could lead to better photocatalytic efficiency under visible light conditions. The retention of the tetragonal crystalline structure upon doping, despite the introduction of Fe3+, highlights a unique stability in the material that could have implications for its durability in practical applications.

The major contributions of the proposed method are as follows,

Iron-doped Zirconia nanoparticles were synthesized using the Co-Precipitation technique. The doping of Fe3+ has shown better photocatalytic degradation efficiency due to the reduction of bandgap.

Iron-doped zirconia exhibits superparamagnetic behavior, according to a VSM investigation.

The anti-microbial properties of Fe3+ doped ZrO2 were studied. The obtained results revealed that the inhibition zone of 24mm for Staph aureus as an anti-bacterial agent and 24mm for Candida parapsilosis as an anti-fungal agent signifying their prospective use as dental filler.

 

Synthesis of pure and Fe-doped ZrO2 nanoparticles

Pure and Fe-doped zirconium oxide nanoparticles were synthesized from chloride aqueous solutions (ZrOCl2.8H2O → Zr4+(aq)+2Cl−(aq)+8H2​O(l), FeCl3→Fe3+(aq)+3Cl−(aq)) and NaOH →Na++OH− act as precipitating agent. The aqueous solution of Zirconium oxychloride and sodium hydroxide was taken in the ratio of 0.5:2. NaOH solution was added drop by drop till the pH value reached 12 and stirred constantly for 2 hours at 60°C. Finally, the obtained precipitate slurry was filtered and washed with deionized water by multiple washing steps and finally with acetone to remove impurities. The ZrO2 thus obtained was annealed at 500°C for 2 hours.

For the synthesis of Zr1-xFexO2 nanoparticles with nominal composition x = 0.04, 0.08, 0.12 wt. %., a calculated amount of Ferric Chloride solution was used. Further, a similar procedure adopted for the preparation of un-doped ZrO2 NPs was followed for the synthesis of Fe-doped ZrO2 NPs. The resultant products are referred to as Fe-1, Fe-2, and, Fe-3 respectively.

 

Photocatalytic activity test

On the degradation of methylene blue (MB), the photocatalytic activity of pure and Fe-doped ZrO2 was investigated. A 0.1M, 50 ml aqueous solution of methylene blue was prepared, and 0.2g of photocatalyst (Fe-1, Fe-2, and Fe-3) was suspended in it. The experiment was carried out in the presence of UV light. The solution is continuously stirred while being exposed to a 50W halogen lamp. Every 60 minutes, 4ml of dye solution was removed from the system, and the dye removal efficiency was determined using a UV-Vis spectrometer.

 

Kirby-Bauer test (KB test)

The KB test, also known as the disc-diffusion antibiotic sensitivity test, is used for the bacterial inhibition experiment. For the development of bacteria, nutrient agar media with a pH of 7.2 was created and inoculated with the experimenting organism. The complete area of antibiotic discs was sprayed with a suspension of gram-positive and gram-negative bacteria. The reference antibiotic is amikacin, which is also spread alongside the disc. The plate was then incubated for 16 hours at 35°C [8,17,18]. In and around the sample, bacterial inhibition zones formed. The diameter of the inhibitory zones was measured after incubation. The agar diffusion method tested the antifungal activity of synthesized materials against Candida Albicans and Candida parapsilosis fungal strains. Nystatin was employed as a reference antifungal. The zone of inhibition is the area where bacterial growth is stopped due to the compound’s bacteriostatic activity, and it is used to assess the compound’s inhibitory impact on a specific microorganism [9-11].

 

Characterization

The structural properties of synthesized nano zirconia, such as crystallite size and phase identification, were validated using an XPERT-PRO diffractometer in the 10o to 80o diffraction angle 2 range. Using a Perkin Elmer Lambda 35 spectrophotometer, UV VIS spectrums for nano ZrO2 were acquired in the wavelength range of 100 to 1100nm. Scanning electron microscope (SEM) and Energy-dispersed X-ray (EDX) with EV018(CARL ZEISS) and Quantax 200 with X Flash 6130 were used to observe the structural morphology and chemical condition. The magnetic characteristics of the produced nanoparticles are studied using Lakeshore Vibrating Sample Magnetometer (VSM) measurements.

 

Results and Discussion

The use of the Co-precipitation method for synthesizing Fe-doped ZrO2 nanoparticles is notable for its simplicity and effectiveness in producing materials with enhanced properties, setting it apart from more traditional synthesis techniques. The various analyses and their findings are interpreted in the following sections.

XRD Analysis

A powder X-ray diffractometer was used to investigate the structural properties of produced materials. Fig. 1 shows the diffraction pattern of pure and iron-doped ZrO2 nanoparticles.

As shown in Fig. 1(a), the XRD pattern of Fe-prepared samples appeared similar to that seen in pure ZrO2 nanoparticles. The presence of sharp and well-defined peaks indicates that the produced samples are highly crystalline. The diffraction peaks are indexed as at 2θ ˜ 30.24º, 34.97º, 35.31º, 50.59º, 59.92º, 63.04º,74.34º, related to the planes (011), (002), (110), (112), (013), (202), (220) respectively are in good agreement with JCPDS card No.50-1089 and match well with the planes of tetragonal structure of ZrO2 nanoparticles, also no impurity peaks are identified in XRD pattern of Fe doped ZrO2 nanoparticles. The retention of the tetragonal crystalline structure upon doping, despite the introduction of Fe3+, highlights a unique stability in the material that could have implications for its durability in practical applications. Compared to pure ZrO2 nanoparticles, the diffraction peaks of iron-doped ZrO2 nanoparticles are somewhat broad and have a slight peak shift towards a higher diffraction angle. As shown in Fig. 1(b) the peak shifts increase as the dopant concentration increases. Thus the Fe ions hold the interstitial lattice sites of ZrO2 nanoparticles.

The lattice characteristics, geometrical parameters, and average crystallite diameters (D) were determined using respective formulas to investigate the effect of Fe content on the crystal properties of produced nanostructures. The crystallite size (D), dislocation density (δ), Stacking Fault (SF), and microstrain (ε) were calculated using equations 1, 2, 3, and 4 respectively. The lattice parameters and the volume of the unit cell are calculated using equations 5 and 6 respectively.

The average crystallite size (D) is calculated using Scherrer’s formula,

                                              (1)

 where ‘λ’ is the wavelength of the X-rays; ‘θ’ is Bragg’s diffraction angle, and ‘β’ is the full width at half maximum (FWHM) of the diffraction peaks (in radians).

The dislocation density (δ) is the length of dislocation per unit volume which depends on the crystallite size (D) and it is calculated using the relation,

                                              (2)

The stacking fault probability is calculated using the formula,

                                 (3)

The microstrain produced due to the dislocations in the nanoparticles is calculated using the relation,

ε                                        (4)

where β is the FWHM and θ is the diffraction angle.

The lattice constants a and c are calculated by using the relation,

 =                           (5)

The volume of ZrO2 and ZrO2-Fe unit cell ‘V’ is calculated by using the relation,

V =                                         (6)

The calculated values are presented in Table 1. There was no discernible pattern of variation in the computed values of crystal properties for produced nanostructures. The ionic size disparity between Zr and Fe could explain the slight fluctuation in the values of lattice constants between un-doped and differentially doped nanostructures. Table 1 shows the relationship between average crystallite size and Fe concentration. The decrease in nucleation and growth rate due to the greater ionic radius of Fe3+ as opposed to Zr2+ was linked to the qualitative decrement of grain size with Fe doping. Shrinkage in crystallite size due to Fe inclusion, as compared to that of un-doped ZrO2, is commonly seen.

 

SEM and EDX Analysis

The influence of Fe doping on the morphology of ZrO2 nanoparticles is analyzed using a scanning electron microscope (SEM). SEM images of un-doped and Fe-doped ZrO2 nanoparticles at different concentrations are shown in Fig.  2(a-d).

The morphology of pure ZrO2 nanoparticles is rod-shaped. Fe-1 has a spherical morphology, while Fe-2 and Fe-3 have a mixture of spherical and needle-shaped morphology with small agglomeration formed. Generally, the agglomeration of particles mainly depends on impurities, reaction rate, charges on the particles, etc. The charge of the particles and the concentration of dopant ions in the host matrix play a role in particle separation. The charge repulsion between the particles is inhibited when the concentration of Fe3+ ions exceeds the crucial value, causing coagulation and particle agglomeration [19,20].

EDX measurement techniques can help to determine the purity and chemical composition of pure and Fe-doped ZrO2 nanoparticles. The EDX spectra of pure and Fe-doped ZrO2 nanoparticles are shown in Fig. 3.

The metal composition was confirmed by EDX characterization. The peaks confirm the presence of iron, zirconium, and oxygen signals. It can be observed that the product is pure and free of any additional contaminants. The elemental composition of Fe-doped ZrO2 nanoparticles is listed in Table 2.

 

UV–Vis Analysis

The structure, morphologies, and chemical states of ZrO2 and its optical absorption characteristics and electrical structure were drastically altered by Fe doping. The UV–Vis absorption spectra of pure and Fe-doped ZrO2 nanoparticles are shown in Fig. 4(a). Fig. 4(a) shows that pure ZrO2 primarily exhibits UV absorption capacity, with the absorption edge positioned at 278.6 nm. Fe-doped ZrO2 samples, on the other hand, have an absorption edge that extends into the visible range and redshifts from 468 nm to 484 nm as the Fe doping amount increases.

The absorbance spectra of Fe-doped ZrO2 samples likewise show an absorption tail, with the absorption peak after 500 nm perhaps induced by the spin-allowed d-d transition of Fe3+ (2T2g        2A2g, 2T1g) [21]. The Tauc plot of pure and Fe-doped ZrO2 is drawn and extrapolating the line to the x-axis energy gap is obtained and it is shown in Figs. 4(b) and 4(c). The band gap energy and the absorption coefficient α are calculated using equations 7 and 8 respectively. 

The band gap energy of the prepared sample is calculated by using the Tauc relation,

                          (7)

where is the energy of a photon,  is the band gap energy, and A is the proportionality constant. n takes the value for direct allowed transitions and    is the absorption coefficient [22]. The absorption coefficient is determined using the formula,

                                     (8)

Here, ‘T’ represents transmittance, and ‘t’ represents the thickness of the sample

The energy gap values of pure and Fe-1, Fe-2, and Fe-3 doped ZrO2 are 4.6 eV, 2.7 eV, 1.8 eV, and 1.6 eV. As per the optical analysis, with the increasing Fe content, the energy gap values were lowered from 4.6 eV to 1.6 eV.  The reduction of the bandgap from 4.6 eV to 1.6 eV is a significant finding, showcasing how Fe doping creates new impurity energy levels that enhance light absorption, which could lead to better photocatalytic efficiency.

 

Photoluminescence Analysis

The photoluminescence spectrum was obtained with an excitation wavelength of 270 nm to explore the emission properties of un-doped and Fe-doped ZrO2 nanoparticles. The photoluminescence (PL) spectra of the pure and Fe-doped ZrO2 samples are shown in Fig. 5.

The PL spectra of pure ZrO2 show peaks at 367 nm, 419 nm, 485 nm, and  542 nm, as seen in Fig. 4. Weak peaks at 367 nm and 419 nm indicated UV emission of pure ZrO2 nanoparticles. In comparison, a sharp and intense peak at    485 nm and a relatively weak peak at 542 nm exhibited blue and green emission of ZrO2 nanoparticles. Compared to pure ZrO2 nanoparticles, the PL spectra of Fe-doped ZrO2 nanoparticles show peaks at 367 nm, 419 nm, 485 nm, 542 nm, and 576 nm with lower intensity. A weaker PL intensity generally indicates a decreased recombination rate of photo-induced carriers. The Fe3+ defect states and the band edge are where the luminous centers of Fe-doped ZrO2 are found [12]. All samples show a PL emission peak at 485 nm after photoexcitation at 270 nm, attributed to intrinsically excited carriers recombining in the conduction and valence bands of ZrO2. For Fe-1, Fe-2, and Fe-3, a second broad PL emission peak at roughly 576 nm is detected compared to pristine ZrO2. Because of the Fe3+ defect states, the 576 nm peak could be attributed to electron transitions from the conduction band edge to deep trap holes. The intensities of Fe-1, Fe-2, and Fe-3 are lower than pristine ZrO2, showing that Fe doping may effectively restrict the recombination rate, which is compatible with the photocatalytic degradation test results [13]. The detailed characterization of defect states provides insights into the underlying mechanisms that enhance photocatalytic activity, representing a novel contribution to the understanding of how doping affects semiconductor properties.

 

Magnetic Properties

The magnetic characteristics of pure and Fe-doped ZrO2 nanoparticles were investigated at ambient temperature using a Vibrating Sample Magnetometer (VSM) with a maximum field of 15000 Oe. The magnetic parameters of pure and Fe-doped ZrO2 nanoparticles are listed in Table 3.

The magnetic hysteresis curve of un-doped and Fe-doped ZrO2 nanoparticles is shown in Fig. 6 (a-d).  For un-doped zirconia, coercivity (Hc) is measured at 2535.6 Oe, saturation magnetization (Ms) is estimated at 0.59 10-3 emu/g, and remanence magnetization (Mr) is measured at 0.054 10-3 emu/g. The hysteresis loop demonstrates perfect Ferromagnetism at Room Temperature (RTFM). For ferromagnetism, a similar M-H loop has been discovered previously [14,15]. Because the synthesized ZrO2 nanoparticle has a high coercivity, it is determined to be a hard ferromagnetic material. To demagnetize the material, more strong magnetic fields are required. Permanent magnetic materials have a magnetic effect in the absence of a magnetic field for an extended period. It is employed in various industries, including telecommunications, data processing, electronics, and instrumentation.

Fig. 6 (b – d) shows that Fe-doped ZrO2 has superparamagnetism behavior. It is confirmed by the magnetic parameters listed in Table 3.  The displacement of Fe3+ ions from the B site to the A site causes the transition from ferro to superparamagnetism of undoped and doped zirconia. The confirmation of superparamagnetic behavior via VSM measurements opens up new avenues for applications in magnetic separation techniques or targeted drug delivery, adding an innovative dimension to the material’s utility. The concentration of Fe3+ ions dropped at the B site while increasing by the same amount at the A site. The lattice’s net magnetization decreases, similar to a previous observation             [16]. The squareness ratio, defined as the ratio of retentivity to saturation magnetization (Mr/Ms), measures how square the hysteresis loop is. This characteristic helps decide which magnetic nanoparticle to utilize for a specific application. In the case of magnetic fluids, it should be as low as feasible.

 

Photo Catalytic Activity

Methylene Blue (MB) dye degradation was used to investigate the photocatalytic performance of pristine and Fe-doped ZrO2 under UV irradiation. The pollutant, MB dye showed negligible degradation after being exposed to UV light for 180 minutes. When Fe-doped Zirconia was added to the same experiment without irradiating UV light, there was no degradation found in the pollutant as a result of the pollutant adsorbing on the catalyst’s surface[25]. The lack of degradation of the pollutant due to the recombination of electron-hole pairs. We found that there was a huge degradation of the pollutant in the presence of both Fe-doped Zirconia and UV irradiation. 

The MB dye degradation curve for un-doped and Fe (0.04 M, 0.08 M, and 0.12 M) doped ZrO2 catalysts with varying time intervals are shown in Fig. 7 (a-d). 

The strong absorption peak of MB is located at 661 nm which is due to the chromophore group. The intensity peak of MB at 661 nm was reduced while increasing the irradiation time. The removal efficiency (E) of MB degradation and the normalized residual concentration of MB dye is estimated using equations 9 and 10 respectively. The following equation provides the removal efficiency (E) of MB degradation,

                       (9)      

where C0 is the initial concentration of dye and C is the concentration of MB after UV irradiation.

The normalized residual concentration of MB dye is estimated using,

                                   (10)

where Co and Ct are the initial and residual concentrations of MB dye. At and Ao are the absorbance intensity at time t and at time t = 0 obtained from the UV-absorbance spectrum.

It was observed that Fe-doped ZrO2 nanoparticles provide faster degradation of MB dye compared to pure ZrO2. 0.12wt% Fe-3 of Fe doped ZrO2 provides 93% degradation within 35 minutes, 0.08wt% (Fe-2) provides 70% and 0.04wt% (Fe-1) provides 48% within 35 minutes.  The normalized residual concentration of MB dye degraded by pure and Fe-doped ZrO2 nanoparticles is shown in Fig. 8 (a,b). The increased photocatalytic activity could be due to more intense absorption of the applied light spectrum by nanoparticles with higher concentrations of Fe3+ ions and oxygen vacancies.

The photocatalytic process begins with the photocatalyst absorbing photons of sufficient energy and the excitation of electrons from the valence band to the conduction band, resulting in the formation of electron/hole pairs. Photo-generated holes can mix with Fe3+ ions in the matrix to form Fe4+, allowing holes to move to the surface and react with adsorbed hydroxyl ions to make hydroxyl radicals. Also, dopant ferric ions (Fe3+) at the surface of doped zirconia particles can react with adsorbed water to generate an aqua complex that can form Fe2+ ions and hydroxyl radicals after UV photon activation. The photocatalytic activity is enhanced by the morphological change and reduction of crystallite size caused by Fe ion doping. According to the findings, Fe-doped (Fe-1, Fe-2, and Fe-3) ZrO2 can effectively enrich photocatalytic activity. Achieving a 93% degradation rate of MB under visible light irradiation within 35 minutes demonstrates the exceptional photocatalytic activity of the Fe-doped ZrO2 nanoparticles, underscoring their potential for real-world environmental applications.

 

Anti-bacterial and Anti-fungal Assessment

Kirby-Bauer (KB) tests evaluated pure and iron-doped Zirconia’s antibacterial and antifungal properties. Gram-positive microorganisms like Bacillus cereus and Staph aureus, as well as gram-negative bacteria like E. coli and Pseudomonas aeruginosa, were tested in the inhibition zone. The anti-bacterial and anti-fungal assessment of Fe-doped ZrO2 nanoparticles is listed in Table 4.

When comparing gram-positive and gram-negative bacteria, the zone of inhibition of pristine ZrO2 was roughly 28 mm. The zone of inhibition for Iron-doped ZrO2 appears to increase as the dopant concentration rises. The most significant zone of inhibition for gram-positive bacteria was around 24 mm, and the maximum area of inhibition for gram-negative bacteria was likewise about 24 mm.

The iron-doped zirconia in Fig. 9 (a-d) has potential against gram-positive and gram-negative microorganisms. From Fig. 9 (e,f) Candida albicans and Candida parapsilosis were both tested for their inhibition zones. In Table 4, the evaluated zone of inhibition values are tabulated. Compared to other fungal pathogens, the highest zone of inhibition obtained for Fe-3 is 24mm for candida parapsilosis.

 

Conclusion

The Co-precipitation method was used to synthesize a series of Fe-doped ZrO2 nanoparticles for photocatalytic and anti-microbial activities. XRD tests validated the tetragonal crystalline structure of pure and doped samples, and the crystal structure did not change when the dopant was absorbed into the host lattice. Fe3+ prompted the tetragonal phase of ZrO2 and the defect states in the bandgap of Fe-doped ZrO2. Defect states extended the light absorption edge of ZrO2, and Fe-doped ZrO2 had a narrow bandgap while maintaining a very negative CB potential. The band gap of the doped samples was lowered from 4.6 eV to 1.6 eV due to the presence of impurity energy levels between CB and VB of ZrO2. Under UV irradiation, the Fe-3 photocatalyst had enhanced photocatalytic activity for MB degradation. The presence of many intraband defect sites (oxygen vacancies, Fe3+/Fe2+, and Fe3+/Fe4+ levels) was confirmed by optical absorption and luminescence studies.  The experimental findings were found to be well-matched to indicate that NPs are superparamagnetic nanoparticles based on VSM measurements. Fe-doped ZrO2 nanoparticles showed the highest photocatalytic activity of 93% under visible light irradiation within 35 min.

 

Conflict of interest:

On behalf of all authors, the corresponding author states that there is no conflict of interest.

 

  1. T. Sakuma, Mater. Sci. Forum 45 (1997) 327-336.https://doi.org/10.1023/A:1006976407047
  1. Yoshida H, Matsui K, Ikuhara Y, J. Am. Ceram. Soc. 5 (2012) 1701-1708vvv. https://doi.org/10.1111/j.1551-2916.2012.05150.x
  2. M. Taguchi, S. Takami, T. Adschiri, T. Nakane, K. Satoa, T. Naka, CrystEngComm Q6 14 (2012) 2132. https://doi.org/10.1039/c2ce06409j
  3. Influence of calcination temperature on structural, optical, dielectric properties of nano zirconium oxide C. Rajababu* Q1 Department of Materials Science and Nano technology, Yogi Vemana University, Kadapa 516003, India
  4. Lerot, L, Legrand, F & Debruycker, P 1991, 'Chemical control in precipitation of spherical zirconia particles', Journal of Materials Science, vol.26, pp.2353-2358. https://doi.org/10.1007/BF01130181
  5. VanCantfort, O, Michaux, B, Pirard, R, Pirard, JP, & Lecloux, AJ 1997, 'Synthesis and characterization of monodisperse spherical zirconia particles',Journal of Sol-Gel Science and Technology,vol. 8,pp. 207-211. https://doi.org/10.1007/BF02436842
  6. Choi,W, Termin,A & Hoffmann, MR 1994, 'The role of metal ion dopants in quantumsized TiO2 correlation between photoreactivity and charge carrier recombination dynamics', Journal of Physics and Chemistry, vol.98,pp. 13669-13679. https://doi.org/10.1021/j100102a038
  7. Luttrell, T., Halpegamage, S., Tao, J. et al. Why is anatase a better photocatalyst than rutile? - Model studies on epitaxial TiO2 films. Sci Rep 4, 4043 (2014). https://doi.org/10.1038/srep04043
  8. Y.-F. Sun, S.-B. Liu, F.-L. Meng, J.-Y. Liu, Z. Jin, L.-T. Kong, J.-H. Liu, Sensors 12, 2610 (2012) https://doi.org/10.3390/s120302610
  9. Jeba, R, Radhika, S, Padma,CM & Ascar Davix, X, 2021, 'Structural, Optical, Thermal, Magnetic Properties of Zirconia Nanorods and their Photocatalytic and Antimicrobial Properties', Journal of Water and Environmental Nanotechnology, vol.6, no.3, pp.252-264.
  10. Jeba, R, Radhika, S, Padma,CM & Ascar Davix, X, 2022, 'Antimicrobial and photocatalytic activities of strontium doped zirconium oxide nanoparticles', Materials Letters, vol. 311,no. 131559. https://doi.org/10.1016/j.matlet.2021.131559
  11. Yalçın, Y, Kılıç,M, & Çınar,Z 2010, 'Fe+3-doped TiO2: a combined experimental and computational approach to the evaluation of visible light activity',AppliedCatalalysisB,vol.99,pp.469-477. https://doi.org/10.1016/j.apcatb.2010.05.013
  12. Qing Cheng, Wulin Yang, Qingling Chen, Jiajun Zhu, Deyi Li, Licai Fu & Lingping Zhou 2020, 'Fe-doped zirconia nanoparticles with highly negative conduction band potential for enhancing visible light photocatalytic performance', Applied Surface Science, vol. 530, no. 147291. https://doi.org/10.1016/j.apsusc.2020.147291
  13. Gurjaspreet Singh, Pawan, Akshpreet Singh, Shilpy, Diksha, Suman, Geetika Sharma, Subash Chandra Sahoo & Amarjit Kaur 2021, 'Propargyl-functionalized single arm allied Anthracene based Schiff bases: Crystal structure, solvatochromism and selective recognition of Fe3+ ion', Journal of Molecular Structure, vol.1229,no.129618. https://doi.org/10.1016/j.molstruc.2020.129618
  14. Ekane Peter Etape, Josepha Foba-Tendo, Lambi John Ngolui, Beckley Victorine Namondo, Fomogne Cyrille Yollande & Marius Borel Nguefack Nguimezong 2018, 'Structural Characterization and Magnetic Properties of Undoped and Ti-Doped ZnO Nanoparticles Prepared by Modified Oxalate Route', Journal of Nanomaterials, Article ID 9072325. https://doi.org/10.1155/2018/9072325
  15. Monisha,P, Priyadharshini,P, Gomathi,SS, & Pushpanathan,K 2021, 'Ferro to superparamagnetic transition: Outcome of Ni doping in polyethylene glycol capped CoFe2O4 nanoparticles, Journal of Alloys and Compounds, vol. 856, no.157447. https://doi.org/10.1016/j.jallcom.2020.157447
  16. Jeba, R, Radhika, S, Padma,CM & Ascar Davix X, 2022, 'Synthesis and characterization of zirconia nanorods as a photo catalyst for the degradation of methylene blue dye', Nanosystems: Physics, Chemistry, Maths, vol.13 (1), pp.78-86. https://doi.org/10.17586/2220-8054-2022-13-1-78-86
  17. Jeba, R, Radhika, S, Padma,CM & Ascar Davix, X, 2022, 'Strontium doped zirconia for enhanced anti-microbial activity', Materials Today: Proceedings,vol.58,pp.927-931. https://doi.org/10.1016/j.matpr.2021.12.226
  18. Gurushantha, K, Anantharaju, KS, Nagabhushana, H, Sharma, SC, Vidya, YS, Shivakumar & Anilkumar, MR 2015, 'Facile green fabrication of iron-doped cubic ZrO2 nanoparticles by Phyllanthus acidus: structural, photocatalytic and photoluminescent properties'. Journal of Molecular Catalysis A: Chemical,no. 397, pp.36-47. https://doi.org/10.1016/j.molcata.2014.10.025
  19. Patel, NH, Deshpande, MP, Bhatt, SV, Patel, KR, & Chaki, SH 2014, 'Structural and magnetic properties of undoped and Mn doped CdS nanoparticles prepared by chemical co-precipitation method', Advanced Materials Letters, vol. 5, pp.671-677. https://doi.org/10.5185/amlett.2014.1574
  20. Carević,MV, Savić,TD, Abazović,ND, Mojović,MD, Novaković,TB & Čomor MI 2020, 'Effect of Fe3+ ion doping on photocatalytic ability of nanozirconia ceramic to degrade 2, 4, 6- trichlorophenol', Ceramics International,vol.46,pp.6820-6827. https://doi.org/10.1016/j.ceramint.2019.11.175
  21. R. Jeba, S. Radhika, C.M. Padma, X. Ascar Davix, The influence of Cu doped ZrO2 catalyst for the modification of the rate of a photoreaction and forming microorganism resistance, J of water and environment Nanotechnology, 7(4): 351-362,2022.
  22. Mehdi Rostami , Hossein Mazaheri , Ali Hassani Joshaghani , Aref Shokri, 'Using Experimental Design to Optimize the Photo-degradation of P-Nitro Toluene by Nano-TiO2 in Synthetic Wastewater', IJE TRANSACTIONS B: Applications Vol. 32, No. 8, (August 2019) 1074-1081. https://doi.org/10.5829/ije.2019.32.08b.03
  23. Shokri, A; Mahanpoor, K; Soodbar, D, 'Degradation Of 2-Nitrophenol From Petrochemical Wastewater By Uv/Nife2o4/Clinoptilolite Process', Fresenius Environmental Bulletin, vol.25,no.2,pp.500-508.
  24. A. Shokri, K. Mahanpoor, 'Using UV/ZnO process for degradation of Acid red 283 in synthetic wastewater', Bulgarian Chemical Communications, Volume 50, Issue 1, (pp. 27 - 32) 2018.