Document Type : Original Research Paper
Graphical Abstract
Introduction
Over recent decades, nanoparticles have been synthesized through a variety of methods, exploring different foundational principles to achieve desired characteristics in terms of size, shape, and functionality [1]. Their distinctive properties, which vary according to size and include thermal, electrical, chemical, and optical attributes, have facilitated their application in diverse sectors such as healthcare and chemical diagnostics [2]. Among the various types of nanoparticles, iron oxides like hematite (α-Fe2O3), maghemite (γ-Fe2O3), goethite (α-FeOOH), and especially magnetite (Fe3O4) have garnered significant attention [3]. Magnetite nanoparticles (MNPs) stand out for their robust applications in biology and medicine due to their biocompatibility, high saturation magnetization, chemical stability, large surface area, and ease of functionalization [4], [5].
The green synthesis method is increasingly recognized in materials science and technology for its environmentally friendly approach to nanoparticle production, emphasizing biocompatible processes that reduce or eliminate the need for harmful chemicals. This method adheres to principles such as waste minimization, decreasing the generation of pollutants, utilizing safer solvents, and relying on renewable resources [6]. Biomaterials derived from various plant components are combined with metal precursors under specific conditions to fabricate nanoparticles, serving roles such as reducing, capping, and stabilizing agents in the synthesis process. The synthesis duration varies based on the plant-derived biochemicals’ type and concentration. While plant extracts are effective in stabilizing and reducing agents for nanoparticle creation, further research into the influence of reaction conditions on synthesis is essential to address challenges in green synthesis methodologies [7]. Capping agents critically influence the characteristics of nanoparticle colloidal suspensions, with colloidal NP efficacy dependent on high suspension stability. Minor adjustments in the solution or to the nanoparticles can greatly impact this stability. Numerous factors, including the solution’s pH, temperature, plant material concentration, reaction time, and specific synthesis protocols, play a role in the green synthesis of nanoparticles. Notably, the choice of plant material significantly dictates the nature and properties of the resulting nanoparticles [8]. Recent preparations of MNPs have utilized natural extracts from leaves of Lagenaria siceraria [9], Laurus nobilis [10], Ficus caricai [11], Pyrus comminis, Azadirachta indica, Pomegranate peel, and Carica papaya. To date, there has been no documented research on the eco-friendly synthesis of iron oxide nanoparticles using extracts from Cocoa bean (Theobroma Cocoa) shells.
The core of MNPs requires a coating of either natural or synthetic coating materials to enable its dispersion in aqueous solutions [12]. Several materials, including polymer molecules, surfactants, and inorganic substances like polyvinylpyrrolidone (PVP), poly (vinyl alcohol) (PVA), polyethylene glycol (PEG), silica, citric acid, dextran, and cetrimonium bromide (CTAB), are recommended to enhance the colloidal and chemical stability of MNPs [13], [14]. PEG stands out as one of the most commonly used surface coating agents for MNPs due to its exceptional biocompatibility, hydrophilicity, ability to prolong the circulation time of MNPs, and enhancement of their colloidal stability [15].
Magnetic hyperthermia therapy (MHT), utilizing MNPs, is a promising approach for cancer treatment. Currently, it is still undergoing clinical trials [16]. For MHT, ferrofluid samples containing MNPs are subjected to an external alternating magnetic field (AMF) to evaluate their heating capabilities, often measured as the specific absorption rate (SAR). The strength of the AMF in MHT can regulate the hyperthermia temperature (TH) as well as influence the properties of MNPs [17]. It is reported that a safe TH for effective cancer treatment ranges from 42°C to 47°C. Within this temperature range, the proteins in the tissue can hydrolyze, leading to acute necrotic death of cancer cells for 30 to 60 minutes. Normal cells remain largely unaffected, thanks to heat transfer phenomena that spare them from the elevated temperatures [16], [18]. It is important to note that MNPs in a low-viscosity medium can induce a magnetic response, where anisotropic particles are physically rotated by the Brownian heating loss mechanism. This process contributes to increases in both the TH and SAR [17].
Statistical experimental designs offer a more straightforward and effective way to optimize functional variables. Among these designs, the Taguchi method is particularly robust and is commonly used in engineering to identify the best process parameters [19], [20], [21]. Over recent years, the Taguchi design method has been applied across various scientific disciplines, including nanotechnology [22], [23]. Numerous research teams have employed this method to prepare and identify key parameters in the formulation of polymeric nanoparticles. For instance, optimization of nanoparticle synthesis has been conducted using chitosan [24], as well as chitosan loaded with carvedilol [25] and poly (D, L-lactide-co-glycolide) loaded with pyrazinamide [26]. Additionally, this technique has been used in developing clove oil nanoemulsions [27] and in the preparation of polylactic acid/groundnut shell nanoparticle biocomposites [28].
The objective of this paper is to identify and optimize the key factors influencing the hydrodynamic size of polymeric particles. Utilizing the Taguchi experimental design methodology, we streamlined the biogenic co-precipitation synthesis of magnetic nanoparticles (MNPs) using Cocoa bean shells (CBS) and the post-synthesis pegylation to produce Pegylated-MNPs. This novel approach integrates Taguchi design with sustainable synthesis methods, focusing on optimizing the hydrodynamic size and evaluating the magnetic hyperthermia properties of the treated nanoparticles. This innovative synthesis route represents a significant advancement in magnetic nanoparticle engineering, offering an efficient methodology for biomedical applications.
Materials and methods
Chemicals
Iron (II) chloride tetrahydrate (FeCl2·4H2O, 99%) and iron (III) chloride hexahydrate (FeCl36H2O, 90%), along with polyethylene glycol (PEG) with a molecular weight of 2000, were used in the synthesis of MNPs and Pegylated-MNPs. These chemicals were procured from Sigma-Aldrich. Additionally, NaOH was sourced from R&M Chemicals. All solutions were prepared using ultrapure water obtained from the Milli-Q® Integral Water Purification System, supplied by Merck Millipore in Darmstadt, Germany.
Preparation of Cocoa Bean Shell Extract
CBS was thoroughly washed with ultrapure water and then air-dried at room temperature. After drying, the shells were cut into fine powder. To prepare the CBS extract, varying concentrations of 10, 15, and 20 g were each added to 100 ml of deionized water. This mixture was then continuously stirred and heated at 80°C for 40 minutes using a magnetic stirrer. Following the heating process, the mixture was filtered using the Whatman no 42 filter paper. The resulting concentrated filtrates, labeled as CBS extract, were then safely stored at refrigeration temperature (4°C) for future use.
Preparation of MNPs
In the initial synthesis process, a plant extract was gradually added to a mixture of Ferric and ferrous salts while stirring at a controlled speed and temperature. Following this, NaOH was added until alkaline pH was reached. The mixture was then stirred, and the color change indicated the formation of MNPs. After the reaction time, the nanoparticles were separated by centrifugation, washed with acetone, and dried in a hot air oven to ensure complete drying before being stored in an airtight container for future use.
Preparation of Pegylated-MNPs
For Pegylated-MNPs, a post-synthesis PEGylation was performed. A solution of PEG was prepared in distilled water with magnetic stirring. Separately, the synthesized MNPs were dispersed in distilled water and then added to the PEG solution. The mixture was stirred for a specific duration at controlled conditions. The sample was then centrifuged, washed with acetone, dried in an oven, and stored in an airtight container for later use.
The parameters for both the green synthesis and PEGylation processes were studied using runs based on the L9 Taguchi model, which will be detailed in the following section.
Taguchi optimization of green synthesis of MNPs and Pegylation of MNPs
In this study, the Taguchi optimization technique was employed to assess the effects of various parameters—concentration of CBS extract, temperature, pH, and stirring speed—on the hydrodynamic size of green-synthesized MNPs. On the other hand, the same optimization technique was used to evaluate the effects of different parameters in the PEGylation process—concentration of PEG polymer, temperature, time, and stirring speed—on the hydrodynamic size of Pegylated-MNPs. Three levels (L) of each parameter were tested, as detailed in Tables 1A and 1B. These levels were established based on values from literature reviews and preliminary experiments. The minimal number of experimental runs required was calculated using the formula shown in (Eq. 1), where N represents the minimum number of experimental runs, P is the number of process parameters, and L is the number of levels per parameter. Consequently, nine experiments were organized into an L9 (34) orthogonal array (OA), as shown in Tables 2A and 2B.
Eq. 1
In the first run of the green synthesis process, shown in Table 2A, 25 mL of 10% CBS extract was gradually added to a mixture of FeCl2·4H2O and FeCl3·6H2O solutions at a 1:2 molar ratio while stirring at 400 RPM and 25°C. Then, 2 M NaOH was added until the pH reached 10. The mixture was stirred for 1 hour. A color change from yellow to intense black indicated the formation and successful synthesis of MNPs. After the contact time ended, the synthesized MNPs were separated by centrifugation at 6000 RPM for 20 minutes. The nanoparticles were then washed twice with acetone. Finally, the nanoparticles were dried in a hot air oven at 80°C for 24 hours to ensure complete drying before being stored in an airtight container for future use. On the other hand, to obtain Pegylated-MNPs, a post-synthesis precipitation PEGylation was performed following the randomized Taguchi runs, as shown in Table 2B. In run 1, 0.5 g of PEG-2000 was dissolved in 50 mL of distilled water with magnetic stirring until fully dissolved. Then, 0.5 g of MNPs was dispersed in 50 mL of distilled water and added to the PEG solution. The mixture was stirred for 30 minutes at 25°C and 400 RPM. The sample was then centrifuged, washed twice with acetone, dried in an oven at 80°C for 24 hours, and stored in an airtight container for later use.
The same procedure was used for both MNPs and Pegylated-MNPs synthesis, which was repeated for runs 2 to 9, maintaining constant stirring time, precursor ratio, plant extract volume, drying temperature, and drying time. The dried nanoparticle samples from runs 1 to 9 were then characterized using dynamic light scattering (DLS) with a Malvern Zetasizer to measure the average particle size, recorded in triplicates. The results were statistically analyzed using Minitab 21 software following the Taguchi experimental design.
Characterization of MNPs and Pegylated-MNPs
MNPs and Pegylated-MNPs were characterized using several analytical instruments, including field emission scanning electron microscopy (FESEM) combined with energy-dispersive X-ray spectroscopy (EDX) (JSM 7600F, JOEL, USA), Zeta potential (ZP) and particle size analyzer (PSA) (Zetasizer Nano ZS90, Malvern, UK), and Fourier-Transform Infrared (FTIR) spectroscopy (spectrum 400, Perkin Elmer, Waltham, MA, USA). The heating efficiency of the samples was tested using the “Nanotherics Magnetherm” system. MNP concentration effects were examined at 170 Oe and 332.8 kHz using 5 mg/ml concentration for both MNPs and Pegylated-MNPs. Samples were dissolved in distilled water, sonicated for 5 minutes, and the temperature was recorded for 15 minutes.
Results and Discussion
Taguchi Optimization Analysis of MNPs and Pegylated-MNPs via Dynamic Light Scattering (DLS)
In this study, we optimized the eco-friendly synthesis of MNPs using CBS plant extract through the Taguchi OA method. This approach was employed to analyze the individual effects of variables such as plant extract concentration, pH, time, and stirring speed on the hydrodynamic size of MNPs. For the PEGylation of MNPs, the investigation focused on assessing the impact of the PEG concentration, time, stirring speed, and temperature on the hydrodynamic size of the same response variable. When MNPs are reduced to smaller sizes, they exhibit superparamagnetic properties, enhancing their performance for many biomedical applications [29], [30]. Additionally, small MNPs with the appropriate hydrodynamic size achieve superior penetration and retention within the body, making them highly suitable for drug delivery applications [31]. This effectiveness is the reason hydrodynamic size is the highlighted response in the Taguchi model. Using the L9 OA Taguchi experimental design, the parametric effects on the hydrodynamic size of MNPs and Pegylated-MNPs were investigated in three replicates. The average Particle size of the MNPs and Pegylated-MNPs, as well as the calculated Signal Noise Ratio (SNR) values for both compounds, were assessed and are displayed in Tables 3A and 3B. This study prioritizes the smaller is better (SNRs) quality characteristic, as the primary goal is to minimize the hydrodynamic size of MNPs and Pegylated-MNPs to enhance drug delivery systems and penetration of the BBB.
Notably, the optimal hydrodynamic size was determined to be 115.6 nm, corresponding to the first run (R1) for MNPs, and 69.19 nm, corresponding to the sixth run (R6) for Pegylated-MNPs. The SNRs for the most optimal sizes for MNPs and Pegylated-MNPs were -41.6 and -36.8, respectively. As illustrated in Fig. 1, there is a noticeable reduction in size from 115.6 nm to 69.18 nm following the pegylation process, suggesting that PEG effectively minimizes aggregation. This size reduction can be attributed to the tendency of PEG molecules to form a coiled structure at low surface densities, effectively wrapping the nanoparticles tightly[32], [33]. The results align with numerous previous studies that have demonstrated the impact of the pegylation process on reducing the hydrodynamic size of synthesized nanoparticles. For instance, a study conducted by Tai et al. reported that the addition of PEG 600 Da to MNPs resulted in a decrease in hydrodynamic size [34]. In a different study by Panday et al. (2020), the incorporation of PEG into PEI-MNPs led to a reduction in size from 93.13 nm to 79.20 nm [35].
For MNPs, it is observed from Table 4A that the parameter with the highest delta value is pH (rank 1), followed by Plant stirring speed (rank 2), Temperature (rank 3), and plant extract conc. (rank 4). This indicates that pH is the most influential parameter in the green synthesis process, while plant extract conc. Is the least influential in this process. The pH parameter appears to be the most influential, as changes in pH can significantly affect the surface zeta potential of the particles. An increase in zeta potential typically reduces the flocculation and aggregation of nanoparticles, enhancing their suspension stability [36], [37], [38]. The optimal pH identified by the model was 10. This specific value and the importance of pH have been discussed extensively in previous studies. For instance, Sun et al. 2007 found that the nucleus growth of MNPs is favored at pH 10 [39]. Similarly, a study by Alzoubi et al. in 2023 showed that among a range from pH 8 to pH 12, a pH of 10 resulted in the formation of the smallest nanoparticle size [40]. Conversely, for Pegylated-MNPs, as shown in Table 4B, the parameter with the highest delta value is stirring speed (rank 1), followed by time (rank 2), PEG conc. (rank 3), and temperature (rank 4). This suggests that stirring speed remains the most critical parameter in the pegylation process, whereas temperature is the least influential. The prominence of stirring speed as a significant factor could be attributed to its effect on increasing the suspension air/interface contact area. This expansion in the contact area leads to enhanced oxygen flow and a reduction in crystal size. Additionally, the influence of stirring speed on particle size contributes to a more uniform solution during the reaction, resulting in narrower particle size distributions. This uniformity is crucial for achieving consistent synthesis outcomes [41].
The contour plots presented in Fig. 2a and 2b elucidate the interactions among process parameters and their effects on the particle size of green synthesized MNPs and Pegylated-MNPs. Stirring speed, as the most influential parameter, is paired with other parameters to assess its impact on particle size. By examining areas that produce desired particle sizes, optimal process conditions can be readily identified. For example, regions distinguished by specific colors on a parameter map indicate the ranges of parameters that lead to a certain particle size. This is essential for standardizing synthesis protocols across both processes. For MNPs, tracking the color corresponding to the optimized size reveals that a stirring speed of 400 rpm, a temperature of 25°C, a pH of 10, and a 10% concentration of plant extract during the green synthesis process result in the smallest nanoparticle size. Conversely, for Pegylated-MNPs, following the color indicative of the optimized size shows that using a stirring speed of 400 rpm for 60 minutes, a temperature of 70°C, and a 2% PEG concentration during the coating process yields the smallest nanoparticle size.
An additional statistical analysis was conducted to assess the impact of process parameters on the Particle size of MNPs and Pegylated-MNPs and to evaluate the error variance using analysis of variance (ANOVA). Tables 5A and 5B display the results of the ANOVA statistical test regarding the effect of process parameters on both processes. The degree of freedom (DF), which represents the number of independent directions a dynamic system can move while adhering to imposed constraints, was determined to be 2 for each parameter. A higher value of the sum of squares (SS) indicates a greater significance of the process parameter [42]. Therefore, in the green synthesis process, the pH parameter, which has the highest SS (2859), is identified as the most influential on the particle size of MNPs, contributing 38% to the variation. Conversely, the plant extract parameter is the least significant, accounting for only a 9% contribution. In the Pegylation process, the stirring speed, with the highest SS (93.38), emerges as the most critical process parameter affecting the particle size of Pegylated-MNPs, contributing 50.83%. Meanwhile, temperature is the least impactful, with an 8.24% contribution.
After analyzing the variation in SNRs, the most advantageous levels for each incubation parameter were determined using the Main effect plot of SNRs for particle size, as illustrated in Fig. 3A and 3B. A pronounced influence of the parameter levels on the particle sizes of both synthesized MNPs and Pegylated-MNPs was evident in these figures. Specifically, the pH of the medium in the green synthesis process emerged as the most influential parameter, as shown in Fig. 3A. Conversely, during the pegylation process, the stirring speed proved to be the most critical factor, as indicated in Fig. 3B. The figures suggest that the optimal conditions for achieving the smallest particle size in green synthesis include a stirring speed of 400 RPM, a pH of 10, a temperature of 25°C, and a plant extract concentration of 10%. For Pegylated-MNPs, the ideal conditions for minimizing particle size during the pegylation process are 400 RPM, a PEG concentration of 3%, a temperature of 70°C, and a stirring duration of 60 minutes.
The optimized parameter levels depicted in Figs. 3A and 3B, along with the contour plots in Figs. 2A and 2B, correspond well with runs R1 for the synthesis of MNPs and R6 for the pegylation process of Pegylated-MNPs. These runs demonstrated the smallest particle sizes and will therefore be implemented during the project for further characterizations and to advance the study.
X-ray diffraction (XRD)
XRD analysis was performed to evaluate the crystal structure and size of both bare and Pegylated-MNPs, as shown in Fig. 4. As expected, both samples exhibited identical patterns. The diffraction peaks at 2θ values of 30.21o, 35.5o, 43.31o, 53.80o, 57.3o, and 62.7o degrees corresponded to the (220), (311), (400), (422), (511), and (440) Bragg angles, aligning closely with the spinel structure of pure magnetite, according to JCPDS card no. 85-1436. A study by [43] found similar XRD patterns that align with the XRD results presented. This demonstrated that the PEG coating did not impact the crystalline structure of magnetite. Additionally, the lower peak intensity observed in the Pegylated-MNPs compared to the bare MNPs suggested the presence of a PEG coating on the surface of the iron oxide nanoparticles. The mean crystallite size was determined using Scherrer’s formula [44], shown in Eq. 2:
Eq. (2)
Here, 𝐷 represents the crystalline domain size, K is the Scherrer constant set at 0.9, 𝜆 is the X-ray wavelength (1.54060 Å or 0.154060 nm), 𝛽 is the peak angular width, and 𝜃 is the diffraction angle, focusing on the most intense peak at (311). The calculated crystallite sizes for the MNPs and Pegylated-MNPs were 10 nm and 11 nm, respectively.
Zeta Potential (ZP)
Assessing the stability of MNPs is a crucial step before their use in any biomedical application. To this end, ZP analysis was conducted to measure the surface charge of both bare and Pegylated-MNPs. As shown in Fig. 5, the ZP values were found to be -40.6±0.65 mV for bare MNPs and -35.7±0.15 mV for Pegylated-MNPs, indicating excellent stability. The primary cause of the negative value is often attributed to the OH- ions associated with the surface of the MNPs when in a pH 10 basic medium. According to the literature, a zeta potential value above ±30 mV suggests high stability in MNPs dispersions [45], [46]. In contrast, a discrete Zeta potential value can lead to particle aggregation and flocculation due to the van der Waals attractive forces acting among iron nanoparticles. This results in the physical instability of the system. These ions can influence the surface charge, potentially leading to reduced stability under certain conditions [47].
The Fourier Transform Infrared (FT-IR)
FT-IR spectroscopy method was employed to verify the successful synthesis of nanoparticles and to identify potential functional groups present on the MNPs, which were synthesized utilizing CBS Extract. FT-IR spectrum of the CBS extract (Fig. 6A) revealed characteristic absorption peaks at 3319, 2918, 1620, and 1251 cm-1. These peaks correspond to the functional groups –OH, =CH–, –C–O, and O–CH, respectively. The presence of these peaks suggests the existence of phenolic compounds such as flavonols, including catechins and procyanidins. These compounds are known to function as reducing agents and stabilizers in the synthesis of MNPs. Additionally, an absorption peak at 1432 cm-1, indicative of C-H bending in -CH2- or -CH3 groups, was observed. Moreover, the peak at 1041 cm-1 is typically associated with C-O stretching vibrations, which could originate from alcohols, ethers, or esters.
In the spectra of MNPs (Fig. 6B) synthesized using the CBS extract, significant changes were noted. The O–CH stretching band at 1251 cm-1 was no longer present, and there was a noticeable shift in the carbonyl band from 1620 to 1608 cm-1. These alterations suggest the coordination of Fe with the carboxylic group. Additionally, a shift in the C-O stretching vibration from 1041 to 1078 cm-1 in the synthesized MNPs was observed, indicating potential interactions when combined with CBS extract. Additionally, the appearance of two distinct peaks at 565 and 582 cm-1, which are associated with the Fe–O bond, confirms the exclusive formation of the magnetite phase. This observation effectively rules out the presence of other iron oxide phases, such as goethite or hematite, in the synthesis [48]. These findings are corroborated by comparing the IR spectrum with those reported in earlier studies [49], [50]. Indeed, the FT-IR spectra of magnetite show prominent bands in the low-frequency range (1000–500 cm-1), which are associated with the iron oxide structure [51], [52].
In the FTIR spectra of Pegylated-MNPs (Fig. 6C), distinct spectral features are observed. The main absorbance peak for the ether stretch band occurs at 1090 cm-1. Bending vibrations of the -CH2 and -CH bands are noted at 1481 cm-1 and 1250 cm-1, respectively, with an additional peak at 980 cm-1. The bending of H-O-H is evident around 1604.6 cm-1. The Fe-O vibration characteristic of Pegylated-MNPs is seen around 565 cm-1. A broad peak spanning from 3500 to 3100 cm-1 across the spectra of CBS Extract, MNPs, and Pegylated-MNPs indicates the presence of attached hydroxyl groups. These observations, including the C-O-C ether stretch, -CH bending, H-O-H bending, and Fe-O stretching, collectively confirm the successful coating of MNPs with PEG on their surface. Table 6 summarizes all the functional groups identified by FTIR and their corresponding wavelengths for the three samples: A) CBS extract, B) MNPs, and C) pegylated-MNPs.
Field Emission-Scanning Electron Microscopy Analysis (FE-SEM)
FE-SEM was employed to examine the morphology of MNPs and Pegylated-MNPs. The images depicted in Fig. 7 reveal spherical nanoparticle clusters that exhibit a high degree of uniformity in size. Furthermore, the images of Pegylated-MNPs demonstrate enhanced dispersion capabilities following the encapsulation process using PEG compared to MNPs alone. This improvement can be attributed to the role of PEG as both a stabilizer and a dispersant [53].
Energy-dispersive X-ray spectroscopy (EDX)
The elemental composition obtained from the EDX analysis is shown in Fig. 8. The weight percentages for the MNPs are approximately 39% O and 61% Fe. In contrast, the Pegylated-MNPs contain 10% C, 31% O, and 59% Fe. Impurities such as aluminum (Al) and chlorine (Cl) in both compounds are present in trace amounts and are considered negligible. The presence of impurities can be minimized by avoiding the use of foil and ensuring that the chemical compounds, FeCl2.4H2O and FeCl3·6H2O, have completely reacted during the synthesis and storage of MNPs before proceeding with FESEM imaging. This careful control of the reaction conditions helps to reduce contamination during the preparation process. Moreover, the detection of sodium (Na), phosphorus (P), and magnesium (Mg) can be attributed to the presence of bioactive molecules from the CBS extract on the surfaces of MNPs and Pegylated-MNPs [54], [55], [56].
Vibrating Sample Magnetometer Analysis (VSM)
Fig. 9 displays the magnetic field versus magnetic moment (M-H) curves for MNPs and Pegylated-MNPs. The VSM curves for these greenly synthesized materials exhibit a sigmoidal shape without a hysteresis loop, demonstrating their superparamagnetic properties. Superparamagnetic properties mean that when exposed to a magnetic field, these nanoparticles tend to aggregate due to magnetic dipole attraction. Importantly, this aggregation is reversible and diminishes upon the removal of the magnetic field, resulting in no residual magnetization. The superparamagnetic nature of these nanoparticles is particularly advantageous for biomedical applications. The saturation magnetization (Ms) values are high, recorded at 18 and 14 emu/g for MNPs and Pegylated-MNPs, respectively. Ms values correlate with the nanoparticles’ small size since Ms typically decreases with particle size reduction, as detailed by Shete and his colleagues. For biomedical purposes, an Ms value in the range of 6–22 emu/g is deemed appropriate [57], [58], [59]. The measured Ms values of 18 and 14 emu/g for MNPs and Pegylated-MNPs respectively fall within this acceptable range, affirming their suitability for biomedical applications. Additionally, both materials exhibit low coercivity, measured at 19.29 and 23.71 Oe, and very low remanence (Mr), with values of 0.63 and 0.33 emu/g for MNPs and Pegylated-MNPs, respectively. The notably low coercive forces and remanence minimize magnetic dipolar interactions among the nanoparticles, significantly reducing the risk of complications, such as blood clots within the circulatory system [60].
Magnetic Hyperthermia Studies
Heating Efficiency
The heating efficiencies of MNPs and Pegylated-MNPs in an alternating current (AC) magnetic field were assessed. Fig. 10 illustrates the temperature increases in MNPs and Pegylated-MNPs dispersed in deionized water at a concentration of 10 mg/ml under an AMF with a frequency of 332.8 kHz and an amplitude of 170 Oe. Key parameters derived from the temperature increase are summarized in Table 7. As depicted in Fig. 10a, MNPs demonstrate robust heating capabilities, achieving magnetic hyperthermia temperatures (42 °C) in relatively brief periods for both formulations. Table 7 indicates that the maximum temperatures for MNPs and Pegylated-MNPs were 50.65°C and 46.03°C, respectively. Both samples achieved the magnetic hyperthermia threshold of 42°C within 15 minutes. Specifically, bare MNPs reached the hyperthermia temperature of 42°C in approximately 7 minutes, whereas Pegylated-MNPs required about 10 minutes to reach the same temperature (referenced in Table 7). This demonstrates that both types of samples are capable of attaining magnetic hyperthermia within relatively short durations. It is crucial to emphasize that for effective magnetic fluid hyperthermia (MFH) treatments, minimal doses of MNPs should be utilized to achieve hyperthermia temperatures rapidly. Therefore, the synthesis of stable, well-dispersed MNPs with high heating efficiencies through an easy, robust, inexpensive, and reproducible method is greatly sought after in the field. Therefore, co-precipitation using green chemistry was employed in the project as a straightforward and non-hazardous approach for synthesizing the desired nanoparticles.
SAR and ILP Measurements
The heat produced by the samples was further quantified using the SAR method [61]. The heat output of the samples was further quantified by SAR, which measures power deposition and evaluates the efficacy of magnetic hyperthermia. SAR can be determined using the calorimetric method as follows:[62]
SAR= (pCw/MassMNP) (ΔT/Δt)
Here, (Cw) represents the specific heat capacity of water (4184 J kg-1 K-1 is the density of the colloid), MassMNPs denotes the concentration of MNPs in the suspension, and ΔT/Δt indicates the rate of heating. By performing a linear regression of the temperature rise against time during the initial period) 1 to approximately 30 seconds), the slope ΔT/Δt is obtained.
The SAR values were recorded at 135 W/g for MNPs and 60 W/g for Pegylated-MNPs, as shown in Fig. 10b. These relatively high values reflect the robust heating capabilities of the synthesized compounds. SAR values were observed to vary based on the core sizes of the nanoparticles, with larger sizes yielding higher SAR values. These findings align with the comprehensive research conducted by [63], which identified a critical nanoparticle size of approximately 12 nm for optimal heating effectiveness. Moreover, [64] demonstrated that synthesizing MNPs, cobalt (Co) MNPs, and nickel (Ni) MNPs using aloe vera plant extract resulted in SAR values of 101, 107, and 103 W/g, respectively. [65]) demonstrated that chemically synthesized, uncoated MNPs had the highest SAR value of 128 W/g. These values are lower than the SAR value reported for bare MNPs in the current research. It appears that there is an ideal size range averaging a core size of about 10-15 nm and a hydrodynamic diameter of 100-150 nm where heat production is maximized. Beyond this optimal size range, the heating efficiency begins to decrease as the hydrodynamic size, viscosity, and polydispersity of the MNP colloid increase. This decrease in efficiency can be attributed to heightened magnetic interparticle dipolar interactions, which lead to a reduction in Neel–Brownian relaxations. Consequently, the nanoparticles are less able to rotate freely under the applied magnetic field, thus diminishing their heating capacity [66]. In addition to SAR values, the maximum temperature achieved and the time required to reach the hyperthermia temperature of 42°C are critical metrics for evaluating the self-heating capabilities of MNPs. Despite these factors, both MNPs and Pegylated-MNPs demonstrated relatively high SAR values and were able to reach hyperthermia temperatures in comparatively short durations. These results underscore the excellent heating efficiencies of these formulations.
Due to the dependence of SAR on extrinsic factors like field amplitude and frequency, comparing SAR values across different materials can be imprecise and inconclusive. ILP has been suggested to facilitate a more accurate comparison of the heating efficiency of the produced PMNPs with other systems. ILP can be calculated using the formula:
ILP = SAR/fH02
Here, f denotes the frequency, and H0 represents the magnetic field strength. The ILP parameter (normalized SAR) considers magnetization losses as independent of frequency within the range typical for hyperthermia treatments (10–1000 kHz).
Table 7 reveals that the intrinsic loss power ILP value for a 5 mg/mL sample of bare MNPs, which is 1.290 nH.m2/kg, exceeds that of the same concentration of Pegylated-MNPs, recorded at 0.694 nH.m2/kg. Moreover, Fig. 10c further demonstrates the high heating efficiency of both samples. Additionally, the ILP values for both types of samples fall within the range commonly reported for commercial ferrofluids, which is between 0.2 and 3.1 nH.m2/kg, underscoring their competitive performance in terms of heating capabilities [67], [68].
Conclusion
The green synthesis of MNPs using CBS extract was successfully performed, followed by its functionalization with PEG. The Taguchi method was used to optimize the parameters, focusing on the particle size of the MNPs and Pegylated-MNPs. The optimal conditions for the green synthesis of MNPs are 10% plant extract concentration, pH 10, stirring speed of 400 RPM, and room temperature (25°C). For the Pegylation of MNPs, the optimal conditions are 2% (w/v) PEG, 60 minutes duration, stirring speed of 600 RPM, and a temperature of 70°C. The hydrodynamic particle sizes obtained were 115 nm for MNPs and 69 nm for Pegylated-MNPs, representing the optimal response. Further statistical analysis showed that the pH value had the most significant impact (38.05%) on the green synthesis of MNPs. In contrast, the stirring speed was the most influential factor (50.83%) in the Pegylation process for Pegylated-MNPs. The FTIR characterization of MNPs and Pegylated-MNPs revealed the presence of Fe–O, as well as CH2 and -CH bands, confirming the PEG coating. Additionally, XRD analysis confirmed the crystalline structure of magnetite. The morphological analysis of the MNPs and Pegylated-MNPs shows a spherical-like structure with uniform dispersion. The heating ability of the MNPs and Pegylated-MNPs was investigated. It was found that both types of nanoparticles could reach hyperthermia temperatures (42°C) in a relatively short time. Interestingly, for MNPs, the highest SAR (135.17 W/g) and ILP (1.29 nHm²/kg) values were achieved, allowing them to reach hyperthermia temperatures in about 7 minutes. For Pegylated-MNPs, the highest SAR (60.18 W/g) and ILP (0.69 nHm²/kg) values were obtained, enabling them to reach hyperthermia temperatures in about 10 minutes. Finally, this study uniquely demonstrates the significant influence of pH on the green synthesis of MNPs and stirring speed on their Pegylation. Furthermore, it highlights the superior heating efficiency and faster hyperthermia induction of the optimized MNPs size compared to optimized Pegylated-MNPs size, supported by their higher SAR and ILP values.
Conflict of Interest
The authors declare no conflict of interest.
Acknowledgments
The authors would like to thank the Deputy Director-General of the Malaysian Cocoa Board (MCB) and the Director of Upstream Technology Cocoa for their permission to publish this paper and for reviewing it. We also appreciate their provision of plant materials for our research. Additionally, we thank the Centre of Foundation Studies for Agricultural Science at Universiti Putra Malaysia in Serdang for their collaboration on this research.